# US 2026/0085387 A1 · Aluminum alloy sheet for can lid

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2026/0085387 A1
- Document ID: US20260085387A1
- Status: Published application
- Kind: A1
- Application number: 19/111,428
- Filed: 2024-04-16
- Published: 2026-03-26
- Earliest claimed: 2023-04-17
- Assignees: Uacj Corporation
- Applicants: UACJ Corporation
- Inventors: Yusuke SATO; Tomotaro EZAKI; Tomoyuki KUDO; Kiyonari TAZOE
- Web page: https://patentgrep.com/patent/US20260085387A1

## CPC

- C22C 21/08: with silicon
- C22F 1/047: of alloys with magnesium as the next major constituent
- C22C: ALLOYS (treatment of alloys C21D, C22F)
- C22F: CHANGING THE PHYSICAL STRUCTURE OF NON-FERROUS METALS AND NON-FERROUS ALLOYS (surface treatment of metallic material involving at least one process provided for in class C23 and at least one process covered by this subclass, C23F17/00)

## Abstract

One aspect of the present disclosure is an aluminum alloy sheet for a can lid including a silicon (Si) content of 0.20 mass % or more and 0.47 mass % or less; an iron (Fe) content of 0.30 mass % or more and 0.70 mass % or less; a copper (Cu) content of 0.11 mass % or more and 0.40 mass % or less; a manganese (Mn) content of 0.70 mass % or more and 1.20 mass % or less; a magnesium (Mg) content of 1.1 mass % or more and 3.7 mass % or less; and a balance consisting of or including aluminum (Al) and inevitable impurities. The aluminum alloy sheet has a solidus temperature higher than a solid solutionizing temperature of Mg2Si.

## Claims

### Claim 1

An aluminum alloy sheet for a can lid, the aluminum alloy sheet comprising:
a silicon (Si) content of 0.20 mass % or more and 0.47 mass % or less;
an iron (Fe) content of 0.30 mass % or more and 0.70 mass % or less;
a copper (Cu) content of 0.11 mass % or more and 0.40 mass % or less;
a manganese (Mn) content of 0.70 mass % or more and 1.20 mass % or less;
a magnesium (Mg) content of 1.1 mass % or more and 3.7 mass % or less; and
a balance consisting of or comprising aluminum (Al) and inevitable impurities,
wherein the aluminum alloy sheet has a solidus temperature higher than a solid solutionizing temperature of Mg2Si.

### Claim 2 (depends on 1)

The aluminum alloy sheet for a can lid according to claim 1,
wherein the aluminum alloy sheet comprising:
a silicon (Si) content of 0.20 mass % or more and 0.47 mass % or less;
an iron (Fe) content of 0.30 mass % or more and 0.59 mass % or less;
a copper (Cu) content of 0.11 mass % or more and 0.40 mass % or less;
a manganese (Mn) content of 0.70 mass % or more and 0.98 mass % or less; and
a magnesium (Mg) content or 1.1 mass % or more and 3.3 mass % or less,
wherein a solidification initiating temperature of Al is higher than a crystallization temperature of a primary crystal.

### Claim 3 (depends on 2)

The aluminum alloy sheet for a can lid according to claim 2,
wherein the aluminum alloy sheet comprising:
a silicon (Si) content of 0.20 mass % or more and 0.39 mass % or less;
an iron (Fe) content of 0.30 mass % or more and 0.59 mass % or less;
a copper (Cu) content of 0.11 mass % or more and 0.40 mass % or less;
a manganese (Mn) content of 0.70 mass % or more and 0.98 mass % or less; and
a magnesium (Mg) content of 1.1 mass % or more and 3.1 mass % or less,
wherein a difference in temperature obtained by deducting a solid solutionizing temperature of Mg2Si from a solidus temperature is 30° C. or more.

### Claim 4 (depends on 3)

The aluminum alloy sheet for a can lid according to claim 3,
wherein the aluminum alloy sheet comprising:
a silicon (Si) content of 0.20 mass % or more and 0.39 mass % or less;
an iron (Fe) content of 0.30 mass % or more and 0.51 mass % or less;
a copper (Cu) content of 0.11 mass % or more and 0.40 mass % or less;
a manganese (Mn) content of 0.70 mass % or more and 0.92 mass % or less; and
a magnesium (Mg) content of 1.1 mass % or more and 2.9 mass % or less,
wherein a difference in temperature obtained by deducting a crystallization temperature of a primary crystal from a solidification initiating temperature of Al is 1° C. or more.