# US 2026/0085384 A1 · High-performance copper alloy tube and preparation method thereof

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2026/0085384 A1
- Document ID: US20260085384A1
- Status: Published application
- Kind: A1
- Application number: 19/403,300
- Filed: 2025-11-28
- Published: 2026-03-26
- Earliest claimed: 2025-07-25
- Assignees: Zhejiang Hailiang Co., Ltd.
- Applicants: Zhejiang Hailiang Co., Ltd.
- Inventors: Lei MENG; Jingbo GAO; Changming WU; Bin DENG; Haidong FU; Luming FENG; Jianguo CAO
- Web page: https://patentgrep.com/patent/US20260085384A1

## CPC

- C22C 9/02: with tin as the next major constituent
- F28F 21/085: {from copper or copper alloys}
- C22C 1/02: by melting {(C22C1/1036 takes precedence)}
- C22F 1/08: of copper or alloys based thereon
- C22C: ALLOYS (treatment of alloys C21D, C22F)
- F28F: DETAILS OF HEAT-EXCHANGE AND HEAT-TRANSFER APPARATUS, OF GENERAL APPLICATION (water and air traps, air venting F16)
- C22F: CHANGING THE PHYSICAL STRUCTURE OF NON-FERROUS METALS AND NON-FERROUS ALLOYS (surface treatment of metallic material involving at least one process provided for in class C23 and at least one process covered by this subclass, C23F17/00)

## Abstract

The present application discloses a high-performance copper alloy tube and a preparation method thereof. In the present application, a copper alloy tube with high strength, high processing and forming capability, excellent pressure resistance, corrosion resistance, and high-temperature softening resistance is prepared by adding Sn, Ni, and P elements to Cu, adjusting the content and proportion of each element, and introducing a high proportion of Σ3, Σ9, and Σ27 coincidence site lattice grain boundaries in combination with recrystallization treatment process. Meanwhile, elements Zr, Co, and B (optionally) are added on the basis of the above alloy components to further improve the performance of the copper alloy tube. The copper alloy tube of the present application meets the performance requirements of the high pressure-resistant and thin-walled seamless copper tube, and has broad application prospects in the field of heat exchange.

## Claims

### Claim 1

A high-performance copper alloy tube, consisting of the following components in mass percentage: 0.05%≤Sn≤0.6%, 0.08%≤Ni<0.3%, 0.015%≤P≤0.045%, and the balance being Cu and unavoidable impurities; and f1=[Sn]+10 [P], f2=[Sn]/[Ni], f1 and f2 satisfying: 0.5%≤f1≤1.05%, 1<f2≤5, wherein [Sn], [P] and [Ni] represent the mass percentage content of Sn, P and Ni, respectively;
the copper alloy tube has a single face-centered cubic crystal structure α phase; the average grain size excluding twin boundaries is 10-25 μm, and the average grain size including twin boundaries is 5-20 μm; the total proportion of Σ3, Σ9, and Σ27 coincidence site lattice grain boundaries in the copper alloy tube is ≥50%, and the ratio of the proportions of Σ9 and Σ27 coincidence site lattice grain boundaries to that of Σ3 coincidence site lattice grain boundaries satisfies: (Σ9+Σ27)/Σ3≤3.5%.

### Claim 2 (depends on 1)

The high-performance copper alloy tube according to claim 1, wherein the copper alloy tube has a tensile strength of ≥260 MPa, a yield-to-tensile ratio of 0.23-0.30, and a burst pressure decay rate of ≤10%; after alternating hot and cold corrosion tests for 21 days in an atmosphere of 0.4% formic acid aqueous solution, a maximum corrosion depth of a single tube is ≤170 μm, and a maximum corrosion depth at a bent portion is ≤190 μm.

### Claim 3 (depends on 1)

The high-performance copper alloy tube according to claim 1, consisting of the following components in mass percentage: 0.05%≤Sn≤0.6%, 0.08%≤Ni<0.3%, 0.015%≤P≤0.045%, and the balance being Cu and unavoidable impurities; and f1=[Sn]+10 [P], f2=[Sn]/[Ni], f1 and f2 satisfying: 0.5%≤f1≤1.05%, 1<f2≤5, wherein [Sn], [P] and [Ni] represent the mass percentage content of Sn, P and Ni, respectively;
the copper alloy tube has a single face-centered cubic crystal structure α phase; the average grain size excluding twin boundaries is 10-25 μm, and the average grain size including twin boundaries is 5-20 μm; the total proportion of Σ3, Σ9, and Σ27 coincidence site lattice grain boundaries in the copper alloy tube is ≥68%, and the ratio of the proportions of Σ9 and Σ27 coincidence site lattice grain boundaries to that of Σ3 coincidence site lattice grain boundaries satisfies: (Σ9+Σ27)/Σ3≥10%.

### Claim 4 (depends on 3)

The high-performance copper alloy tube according to claim 3, wherein the copper alloy tube has a tensile strength of ≥285 MPa, a yield-to-tensile ratio of 0.21-0.28, and a burst pressure decay rate of ≤5%; after alternating hot and cold corrosion tests for 21 days in an atmosphere of 0.4% formic acid aqueous solution, a maximum corrosion depth of a single tube is ≤155 μm, and a maximum corrosion depth at a bent portion is ≤165 μm.

### Claim 5

A high-performance copper alloy tube, consisting of the following components in mass percentage: 0.05%≤Sn≤0.6%, 0.08%≤Ni<0.3%, 0.015%≤P≤0.045%, 0.001%≤Zr<0.03%, 0.001%≤Co<0.01%, 0≤B<0.01%, and the balance being Cu and unavoidable impurities; and f1=[Sn]+10 [P]+10 [Zr], f2=[Sn]/[Ni], f1 and f2 satisfying: 0.65%≤f1<1.15%, 1<f2≤5, wherein [Sn], [P], [Zr], and [Ni] represent the mass percentage content of Sn, P, Zr and Ni, respectively;
the copper alloy tube has a single face-centered cubic crystal structure α phase; the average grain size excluding twin boundaries is 10-25 μm, and the average grain size including twin boundaries is 5-20 μm; the total proportion of Σ3, Σ9, and Σ27 coincidence site lattice grain boundaries in the copper alloy tube is ≥60%, and the ratio of the proportions of Σ9 and Σ27 coincidence site lattice grain boundaries to that of Σ3 coincidence site lattice grain boundaries satisfies: (Σ9+Σ27)/Σ3≤4.0%.

### Claim 6 (depends on 5)

The high-performance copper alloy tube according to claim 5, wherein the copper alloy tube has a tensile strength of ≥275 MPa, a yield-to-tensile ratio of 0.22-0.29, and a burst pressure decay rate of ≤6%; after alternating hot and cold corrosion tests for 21 days in an atmosphere of 0.4% formic acid aqueous solution, a maximum corrosion depth of a single tube is ≤165 μm, and a maximum corrosion depth at a bent portion is ≤180 μm.

### Claim 7 (depends on 5)

The high-performance copper alloy tube according to claim 5, wherein 0.001%≤B<0.01%.

### Claim 8 (depends on 7)

The high-performance copper alloy tube according to claim 7, wherein after alternating hot and cold corrosion tests of the copper alloy tube for 21 days in an atmosphere of 0.4% formic acid aqueous solution, a maximum corrosion depth of a single tube is ≤155 μm, and a maximum corrosion depth at a bent portion is ≤170 μm.

### Claim 9 (depends on 5)

The high-performance copper alloy tube according to claim 5, consisting of the following components in mass percentage: 0.05%≤Sn≤0.6%, 0.08%≤Ni<0.3%, 0.015%≤P≤0.045%, 0.001%≤Zr<0.03%, 0.001%≤Co<0.01%, 0≤B<0.01%, and the balance being Cu and unavoidable impurities; and f1=[Sn]+10 [P]+10 [Zr], f2=[Sn]/[Ni], f1 and f2 satisfying: 0.65%≤f1<1.15%, 1<f2≤5, wherein [Sn], [P], [Zr], and [Ni] represent the mass percentage content of Sn, P, Zr and Ni, respectively;
the copper alloy tube has a single face-centered cubic crystal structure α phase; the average grain size excluding twin boundaries is 10-25 μm, and the average grain size including twin boundaries is 5-20 μm; the total proportion of Σ3, Σ9, and Σ27 coincidence site lattice grain boundaries in the copper alloy tube is ≥72%, and the ratio of the proportions of Σ9 and Σ27 coincidence site lattice grain boundaries to that of Σ3 coincidence site lattice grain boundaries satisfies: (Σ9+ΣΣ7)/Σ3≥12%.

### Claim 10 (depends on 9)

The high-performance copper alloy tube according to claim 9, wherein the copper alloy tube has a tensile strength of ≥295 MPa, a yield-to-tensile ratio of 0.20-0.27, and a burst pressure decay rate of ≤2%; after alternating hot and cold corrosion tests for 21 days in an atmosphere of 0.4% formic acid aqueous solution, a maximum corrosion depth of a single tube is ≤150 μm, and a maximum corrosion depth at a bent portion is ≤160 μm.

### Claim 11 (depends on 9)

The high-performance copper alloy tube according to claim 9, wherein 0.001%≤B<0.01%.

### Claim 12 (depends on 11)

The high-performance copper alloy tube according to claim 11, wherein after alternating hot and cold corrosion tests of the copper alloy tube for 21 days in an atmosphere of 0.4% formic acid aqueous solution, a maximum corrosion depth of a single tube is ≤145 μm, and a maximum corrosion depth at a bent portion is ≤155 μm.

### Claim 13 (depends on 1)

A preparation method of the high-performance copper alloy tube according to claim 1, comprising the following:
batching and smelting: smelting the raw materials meeting the content and ratio;
continuous casting: continuously casting the molten liquid to obtain a billet;
rolling: rolling the billet to obtain a rolled tube blank;
combined drawing: reducing the diameter of the rolled tube blank;
recrystallization treatment: obtaining a product with target properties by controlling the deformation amount and annealing parameters.

### Claim 14 (depends on 13)

The preparation method of the high-performance copper alloy tube according to claim 13, wherein the recrystallization treatment is a single recrystallization process, which is “block drawing→final annealing” with a total deformation amount of block drawing not less than 80%, a final annealing temperature of 500-750° C., and an annealing time of 30-150 min.

### Claim 15 (depends on 13)

The preparation method of the high-performance copper alloy tube according to claim 13, wherein the recrystallization treatment is repeated recrystallization, which is performed for multiple cycles of “block drawing→annealing” after 1-3 passes of block drawing, with a total deformation amount of the 1-3 passes of block drawing before the cycles≤72%; in the multiple cycles of “block drawing→annealing”, a number of cycles is 3-6, a deformation amount of block drawing per cycle is 25-35%, an annealing temperature is 500-600° C., and an annealing time is 10-70 min.

### Claim 16 (depends on 5)

A preparation method of the high-performance copper alloy tube according to claim 5, comprising the following:
batching and smelting: smelting the raw materials meeting the content and ratio;
continuous casting: continuously casting the molten liquid to obtain a billet;
rolling: rolling the billet to obtain a rolled tube blank;
combined drawing: reducing the diameter of the rolled tube blank;
recrystallization treatment: obtaining a product with target properties by controlling the deformation amount and annealing parameters.

### Claim 17 (depends on 16)

The preparation method of the high-performance copper alloy tube according to claim 16, wherein the recrystallization treatment is a single recrystallization process, which is “block drawing→final annealing” with a total deformation amount of block drawing not less than 80%, a final annealing temperature of 500-750° C., and an annealing time of 30-150 min.

### Claim 18 (depends on 16)

The preparation method of the high-performance copper alloy tube according to claim 16, wherein the recrystallization treatment is repeated recrystallization, which is performed for multiple cycles of “block drawing→annealing” after 1-3 passes of block drawing, with a total deformation amount of the 1-3 passes of block drawing before the cycles≤72%; in the multiple cycles of “block drawing→annealing”, a number of cycles is 3-6, a deformation amount of block drawing per cycle is 25-35%, an annealing temperature is 500-600° C., and an annealing time is 10-70 min.