# US 2026/0076241 A1 · Method for manufacturing sinter bonding film, and method for manufacturing power semiconductor package

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2026/0076241 A1
- Document ID: US20260076241A1
- Status: Published application
- Kind: A1
- Application number: 19/106,644
- Filed: 2023-03-23
- Published: 2026-03-12
- Earliest claimed: 2022-09-01
- Assignees: Foundation for Research and Business, Seoul National University of Science and Technology
- Applicants: Foundation for Research and Business, Seoul National University of Science and Technology
- Inventors: Jonghyun LEE; Woo Lim CHOI
- Web page: https://patentgrep.com/patent/US20260076241A1

## CPC

- H10W 72/013: {of die-attach connectors}
- H10W 72/073: {of die-attach connectors}
- H10W 72/30: Die-attach connectors
- H10W 99/00: Subject matter not provided for in other groups of this subclass
- H10W 72/01333: {in liquid form, e.g. spin coating, spray coating or immersion coating}
- H10W 72/01361: {Chemical or physical modification, e.g. by sintering or anodisation (patterning H10W72/01351)}
- H10W 72/01365: {Thermally treating (reflowing H10W72/01357)}
- H10W 72/07331: {Connecting techniques}
- H10W 72/07332: {Compression bonding, e.g. thermocompression bonding}
- H10W 72/325: {Die-attach connectors having a filler embedded in a matrix}
- H10W 72/352: {comprising metals or metalloids, e.g. solders}
- H10W 72/354: {comprising polymers}
- H10W 72/951: {Materials of bond pads}
- H10W: GENERIC PACKAGES, INTERCONNECTIONS, CONNECTORS OR OTHER CONSTRUCTIONAL DETAILS OF DEVICES COVERED BY CLASS H10

## Abstract

A method for manufacturing sinter bonding film, includes: preparing a resin formulation; preparing a metal filler mixture; mixing the resin formulation and the metal filler mixture, thereby preparing a paste for film manufacturing; and manufacturing a sinter bonding film by using the paste for film manufacturing. The metal filler mixture includes a metal powder and a reducing agent, copper metal (Cu) corresponds to respective particles in the metal powder, and the surface of the respective particles in the metal powder undergoes acid treatment or non-treatment.

## Claims

### Claim 1

A method of forming a sinter-bonding film comprising:
preparing a resin formulation;
preparing a metal filler mixture;
mixing the resin formulation with the metal filler mixture to prepare a film-forming paste; and
forming a sinter-bonding film using the film-forming paste,
wherein the metal filler mixture comprises:
a metal powder; and
a reducing agent,
wherein a copper (Cu) metal corresponds to respective particles of the metal powder and
a surface of each particle in the metal powder is subjected to acid treatment or non-treatment.

### Claim 2 (depends on 1)

The method according to claim 1, wherein the preparing a resin formulation comprises:
filling a first container with a resin;
pouring a resin solvent into the resin in the first container; and
dissolving the resin using the resin solvent to prepare a resin formulation,
wherein the resin and the resin solvent are mixed in a weight ratio of 1:2 to 1:5 in the first container.

### Claim 3 (depends on 2)

The method according to claim 2, wherein the resin is an acrylate polymer including at least one of polymethyl acrylate (PMA), polyethyl acrylate (PEA), poly(n-butyl acrylate) (PnBA), poly(2-ethylhexyl acrylate) (PEHA), or poly(2-hydroxyethyl acrylate) (PHEA), or a methacrylate polymer including at least one of polymethyl methacrylate (PMMA), poly(N-butyl methacrylate) (PnBMA), poly(iso-butyl methacrylate) (PIBMA), poly(2-hydroxyethyl methacrylate) (PEHMA), polyhydroxyethylmethacrylate (PHEMA), or poly(N,N-dimethylamino) ethyl methacrylate (PDMAEMA).

### Claim 4 (depends on 2)

The method according to claim 2, wherein the resin solvent is a ketone solvent including at least one of acetone or methyl ethyl ketone (MEK), a dipolar aprotic solvent including at least one of N-methyl pyrrolidone (NMP), dimethyl acetamide (DMAC), dimethyl formamide (DMF), or dimethyl sulfoxide (DMSO), an aromatic hydrocarbon including at least one of benzene or toluene, or chloroform, isopropanol, or tetrahydrofuran (THF).

### Claim 5 (depends on 2)

The method according to claim 2, wherein the preparing a metal filler mixture comprises:
filling the second container with the metal powder; and
pouring the reducing agent into the metal powder in the second container,
wherein the metal powder comprises first metal particles having a first particle size, or comprises first metal particles having a first particle size and second metal particles having a second particle size larger than the first particle size, and
the metal powder is prepared by mixing the first metal particles with the second metal particles in a volume ratio of 100:0 to 26:74.

### Claim 6 (depends on 5)

The method according to claim 5, wherein each of the first metal particles has a particle size of 100 nm to 900 nm and
each of the second metal particles has a particle size of 1.5 μm to 25 μm.

### Claim 7 (depends on 5)

The method according to claim 5, wherein the reducing agent includes at least one of ethylene glycol, diethylene glycol, triethylene glycol (TEG), tetraethylene glycol (TTEG), polyethylene glycol (PEG), propylene glycol, dipropylene glycol, tripropylene glycol, polypropylene glycol, glycerol, 1,4-butanediol, 1,5-pentanediol, α-terpineol, diethyl toluene diamine, diethanol amine, or triethanol amine.

### Claim 8 (depends on 5)

The method according to claim 5, wherein the preparing a film-forming paste comprises:
pouring the resin formulation of the first container into the metal filler mixture of the second container; and
mixing the metal filler mixture with the resin formulation in the second container,
wherein the film-forming paste comprises:
6 to 10 parts by weight of the resin;
18 to 30 parts by weight of the resin solvent; and
0.5 to 2 parts by weight of the reducing agent,
with respect to 100 parts by weight of the metal filler mixture.

### Claim 9 (depends on 8)

The method according to claim 8, wherein the forming a sinter-bonding film comprises:
pouring the film-forming paste of the second container onto a preliminary carrier film;
spreading the film-forming paste thinly on the preliminary carrier film through a blade while moving the preliminary carrier film using a doctor blade device, or spreading the film-forming paste thinly on the preliminary carrier film through a squeegee while fixing the preliminary carrier film using a screen printing device;
drying the film-forming paste on the preliminary carrier film at a temperature of 75° C. to 120° C. for 1 minute to 5 minutes to form a preliminary sinter-bonding film; and
cutting the preliminary carrier film and the preliminary sinter-bonding film into a predetermined size, or ripping the preliminary sinter-bonding film on the preliminary carrier film into a predetermined size.

### Claim 10 (depends on 9)

The method according to claim 9, wherein the reducing agent and the resin are left along with the metal powder in the preliminary sinter-bonding film after drying the film-forming paste,
the reducing agent surrounds the surface of each particle in the metal powder and reduces the oxide layer on the surface of each particle after drying the film-forming paste,
the resin is disposed between respective particles in the metal powder after drying the film-forming paste to connect the particles, and
the resin solvent is removed from the preliminary sinter-bonding film while drying of the film-forming paste.

### Claim 11 (depends on 2)

The method according to claim 2, wherein the preparing a metal filler mixture comprises:
filling a second container with a metal powder;
pouring a carboxyl group-containing acid into the metal powder in the second container to acid-treat the surface of each particle of the metal powder using the carboxyl group-containing acid; and
pouring the reducing agent into the metal powder in the second container,
wherein the metal powder comprises first metal particles having a first particle size, or comprises first metal particles having a first particle size and second metal particles having a second particle size larger than the first particle size,
the metal powder is prepared by mixing the first metal particles with the second metal particles in a volume ratio of 100:0 to 26:74, and
the carboxyl group-containing acid comprises 1 to 5 parts by weight of the carboxylic acid with respect to 100 parts by weight of the alcohol in the second container.

### Claim 12 (depends on 11)

The method according to claim 11, wherein each first metal particle has a particle size of 100 nm to 900 nm and
each second metal particle has a particle size of 1.5 μm to 25 μm.

### Claim 13 (depends on 11)

The method according to claim 11, wherein the carboxylic acid comprises at least one of formic acid, acetic acid, oxalic acid, malic acid, malonic acid, stearic acid, or succinic acid.

### Claim 14 (depends on 11)

The method according to claim 11, wherein each particle in the metal powder has a rough shape after acid-treating the surface of each particle in the metal powder using the carboxyl group-containing acid.

### Claim 15 (depends on 11)

The method according to claim 11, wherein the reducing agent comprises at least one of ethylene glycol, diethylene glycol, triethylene glycol (TEG), tetraethylene glycol (TTEG), polyethylene glycol (PEG), propylene glycol, dipropylene glycol, tripropylene glycol, polypropylene glycol, glycerol, 1,4-butanediol, 1,5-pentanediol, α-terpineol, diethyl toluene diamine, diethanol amine, or triethanol amine.

### Claim 16 (depends on 11)

The method according to claim 11, wherein the preparing a film-forming paste comprises:
pouring the resin formulation of the first container into the metal filler mixture of the second container; and
mixing the metal filler mixture with the resin formulation in the second container,
wherein the film-forming paste comprises:
6 to 10 parts by weight of the resin;
18 to 30 parts by weight of the resin solvent; and
0.5 to 2 parts by weight of the reducing agent,
with respect to 100 parts by weight of the metal filler mixture.

### Claim 17 (depends on 16)

The method according to claim 16, wherein the forming a sinter-bonding film comprises:
pouring the film-forming paste of the second container onto a preliminary carrier film; and
spreading the film-forming paste thinly on the preliminary carrier film through a blade while moving the preliminary carrier film using a doctor blade device, or spreading the film-forming paste thinly on the preliminary carrier film through a squeegee while fixing the preliminary carrier film using a screen printing device;
drying the film-forming paste on the preliminary carrier film at a temperature of 75° C. to 120° C. for 1 minute to 5 minutes to form a preliminary sinter-bonding film; and
cutting the preliminary carrier film and the preliminary sinter-bonding film into a predetermined size, or ripping the preliminary sinter-bonding film on the preliminary carrier film into a predetermined size.

### Claim 18 (depends on 17)

The method according to claim 17, wherein the reducing agent and the resin are left along with the metal powder in the preliminary sinter-bonding film after drying the film-forming paste,
the reducing agent surrounds the surface of each particle in the metal powder along with the carboxyl group-containing acid and reduces the oxide layer on the surface of each particle after drying the film-forming paste,
the resin is disposed between respective particles in the metal powder after drying the film-forming paste to connect the particles, and
the resin solvent is removed from the preliminary sinter-bonding film after drying of the film-forming paste.

### Claim 19

A method of manufacturing a power semiconductor package comprising:
preparing a first bonding subject on a heating stage;
sequentially placing a sinter-bonding film and a second bonding subject on the first bonding subject; and
applying a thermal compression sinter-bonding process to the first bonding subject, the sinter-bonding film and the second bonding subject,
wherein the sinter-bonding film is formed using a metal filler mixture and a resin formulation before the thermal compression sinter-bonding process,
the metal filler mixture comprises a metal powder and a reducing agent,
a copper (Cu) metal is applied to each particle in the metal powder, and
a surface of each particle in the metal powder is subjected to acid treatment or non-treatment.

### Claim 20 (depends on 19)

The method according to claim 19, wherein the metal powder comprises first metal particles having a first particle size, or comprises first metal particles having a first particle size and second metal particles having a second particle size larger than the first particle size,
each of the first metal particles has a particle size of 100 nm to 900 nm and each of the second metal particles has a particle size of 1.5 μm to 25 μm, and
the metal powder is prepared by mixing the first metal particles with the second metal particles in a volume ratio of 100:0 to 26:74.

### Claim 21 (depends on 19)

The method according to claim 19, wherein the metal powder comprises first metal particles having a first particle size, or comprises first metal particles having a first particle size and second metal particles having a second particle size larger than the first particle size,
each of the first metal particles has a particle size of 100 nm to 900 nm and each of the second metal particles has a particle size of 1.5 μm to 25 μm,
the metal powder is prepared by mixing the first metal particles with the second metal particles in a volume ratio of 100:0 to 26:74, and
the surface of each first metal particle is acid-treated using the carboxyl group-containing acid or the surface of each first metal particle and each second metal particle is acid-treated using the carboxyl group-containing acid.

### Claim 22 (depends on 21)

The method according to claim 21, wherein the carboxyl group-containing acid comprises 1 to 5 parts by weight of carboxylic acid with respect to 100 parts by weight of alcohol, and
the carboxylic acid comprises at least one of formic acid, acetic acid, oxalic acid, malic acid, malonic acid, stearic acid, or succinic acid.

### Claim 23 (depends on 21)

The method according to claim 21, wherein each particle in the metal powder has a rough shape after acid-treatment of the surface of each particle in the metal powder using the carboxyl group-containing acid.

### Claim 24 (depends on 19)

The method according to claim 19, wherein the resin is an acrylate polymer including at least one of polymethyl acrylate (PMA), polyethyl acrylate (PEA), poly(n-butyl acrylate) (PnBA), poly(2-ethylhexyl acrylate) (PEHA), or poly(2-hydroxyethyl acrylate) (PHEA), or is a methacrylate polymer including at least one of polymethyl methacrylate (PMMA), poly(N-butyl methacrylate) (PnBMA), poly(iso-butyl methacrylate) (PIBMA), poly(2-hydroxyethyl methacrylate) (PEHMA), polyhydroxyethylmethacrylate (PHEMA), or poly(N,N-dimethylamino) ethyl methacrylate (PDMAEMA), and
the resin is disposed between the respective particles in the metal powder to connect the particles.

### Claim 25 (depends on 19)

The method according to claim 19, wherein the reducing agent comprises at least one of ethylene glycol, diethylene glycol, triethylene glycol (TEG), tetraethylene glycol (TTEG), polyethylene glycol (PEG), propylene glycol, dipropylene glycol, tripropylene glycol, polypropylene glycol, glycerol, 1,4-butanediol, 1,5-pentanediol, α-terpineol, diethyl toluene diamine, diethanol amine, or triethanol amine, and
the reducing agent surrounds the surface of each particle in the metal powder and reduces the oxide layer on the surface of each particle during the thermal compression sinter-bonding process.

### Claim 26 (depends on 19)

The method according to claim 19, wherein the preparing the first bonding subject on the heating stage comprises:
placing a first tray containing a plurality of first bonding subjects around the heating stage; and
placing the first bonding subject from the first tray on the heating stage using a first pick-up tool,
wherein the first bonding subject comprises a direct bonded copper (DBC) substrate or an active brazing ceramic substrate, which comprises a first copper layer, a metal oxide substrate layer, and a second copper layer that are sequentially laminated.

### Claim 27 (depends on 19)

The method according to claim 19, wherein the sequentially placing the sinter-bonding film and the second bonding subject on the first bonding subject comprises:
placing a second tray containing a plurality of unit laminates, each including the sinter-bonding film and the carrier film, around the heating stage;
placing a third tray containing a plurality of second bonding subjects around the heating stage;
placing the sinter-bonding film and the carrier film on the first bonding subject from the second tray using a second pick-up tool;
separating the carrier film from the sinter-bonding film; and
placing the second bonding subject on the sinter-bonding film from the third tray using a third pick-up tool.

### Claim 28 (depends on 27)

The method according to claim 27, wherein the applying the thermal compression sinter-bonding process to the first bonding subject, the sinter-bonding film and the second bonding subject comprises bonding the first and second bonding subjects to the sinter-bonding film while performing the thermal compression sinter-bonding process on the first bonding subject, the sinter-bonding film, and the second bonding subject using the heating stage and the third pick-up tool, and
the thermal compression sinter-bonding process is performed in an air atmosphere or a nitrogen atmosphere at a temperature of 300° C. to 370°C. for a time of 10 seconds to 60 seconds, and at a pressure of 0.5 MPa to 15 MPa.

### Claim 29 (depends on 28)

The method according to claim 28, wherein the first and second bonding subjects are bonded to the sinter-bonding film using at least one of silver (Ag), gold (Au), copper (Cu), or nickel (Ni) as a surface metal layer of the first and second bonding subjects, and
the second bonding subject comprises a power semiconductor chip of a wide band gap compound.

### Claim 30 (depends on 28)

The method according to claim 28, wherein the sinter-bonding film reduces the oxide layer present on the surface of each particle in the metal powder through the reducing agent to remove the oxide layer from the surface during the thermal compression sinter-bonding process and removes the residual resin through an ignition reaction of the film.

### Claim 31 (depends on 19)

The method according to claim 19, wherein the sequentially placing the sinter-bonding film and the second bonding subject on the first bonding subject further comprises:
placing a second tray containing a plurality of second bonding subjects around the heating stage;
placing a third tray containing a large laminate material including an uncut preliminary sinter-bonding film and a preliminary carrier film around the heating stage;
picking up the second bonding subject from the second tray using a fourth pick-up tool;
placing the second bonding subject on the preliminary sinter-bonding film and the preliminary carrier film the third tray using the fourth pick-up tool, and ripping the sinter-bonding film from the preliminary sinter-bonding film in the shape of the second bonding subject while contacting under pressure by stamping the second bonding subject on the preliminary sinter-bonding film to transfer the sinter-bonding film to the lower part of the second bonding subject; and
placing the second bonding subject combined with the sinter-bonding film on the first bonding subject using the fourth pick-up tool and performing thermal compression sintering.

### Claim 32 (depends on 31)

The method according to claim 31, wherein the applying the thermal compression sinter-bonding process to the first bonding subject, the sinter-bonding film and the second bonding subject comprises bonding the first and second bonding subjects to the sinter-bonding film while performing the thermal compression sinter-bonding process on the first bonding subject, the sinter-bonding film, and the second bonding subject using the fourth pick-up tool and the heating stage, and
the thermal compression sinter-bonding process is performed in an air atmosphere or a nitrogen atmosphere at a temperature of 300° C. to 370°C. for a time of 10 seconds to 60 seconds, and at a pressure of 0.5 MPa to 15 MPa.

### Claim 33 (depends on 32)

The method according to claim 32, wherein the first and second bonding subjects are bonded to the sinter-bonding film using at least one of silver (Ag), gold (Au), copper (Cu), or nickel (Ni) as a surface metal layer of the first and second bonding subjects, and
the second bonding subject comprises a power semiconductor chip of a wide band gap compound.

### Claim 34 (depends on 32)

The method according to claim 32, wherein the sinter-bonding film reduces the oxide layer present on the surface of each particle in the metal powder through the reducing agent during the thermal compression sinter-bonding process to remove the oxide layer from the surface and remove the residual resin through an ignition reaction of the film.