# US 2026/0074215 A1 · Positive Electrode Active Material, and Positive Electrode and Lithium Secondary Battery Including the Same

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2026/0074215 A1
- Document ID: US20260074215A1
- Status: Published application
- Kind: A1
- Application number: 19/108,339
- Filed: 2023-12-22
- Published: 2026-03-12
- Earliest claimed: 2022-12-26
- Assignees: LG Energy Solution, Ltd.
- Applicants: LG Energy Solution, Ltd.
- Inventors: Min Kwak; Hyeong Il Kim; Seul Ki Chae; Byung Chun Park
- Web page: https://patentgrep.com/patent/US20260074215A1

## CPC

- H01M 4/525: of mixed oxides or hydroxides containing iron, cobalt or nickel for inserting or intercalating light metals, e.g. LiNiO2, LiCoO2 or LiCoOxFy
- C01G 53/506: with the molar ratio of nickel with respect to all the metals other than alkali metals higher than or equal to 0.8, e.g. Li(MzNixCoyMn1-x-y-z)O2 with x ≥ 0.8
- H01M 4/505: of mixed oxides or hydroxides containing manganese for inserting or intercalating light metals, e.g. LiMn2O4 or LiMn2OxFy
- H01M 10/052: Li-accumulators
- H01M 10/0525: Rocking-chair batteries, i.e. batteries with lithium insertion or intercalation in both electrodes; Lithium-ion batteries
- C01P 2004/32: Spheres
- C01P 2004/53: bimodal size distribution
- C01P 2004/61: Micrometer sized, i.e. from 1-100 micrometer
- H01M 2004/021: {Physical characteristics, e.g. porosity, surface area}
- H01M 2004/028: {Positive electrodes}
- Y02E 60/10: Energy storage using batteries
- H01M: PROCESSES OR MEANS, e.g. BATTERIES, FOR THE DIRECT CONVERSION OF CHEMICAL ENERGY INTO ELECTRICAL ENERGY
- C01G: COMPOUNDS CONTAINING METALS NOT COVERED BY SUBCLASSES C01D OR C01F (metal hydrides {monoborane, diborane or addition complexes thereof} C01B6/00; salts of oxyacids of halogens C01B11/00; peroxides, salts or peroxyacids C01B15/00; thiosulfates, dithionites, polythionates C01B17/64; compounds containing selenium, or tellurium C01B19/00; binary compounds of nitrogen with metals C01B21/06; azides C01B21/08; {compounds containing nitrogen, other non-metals and metal C01B21/082}; metal amides C01B21/092; nitrites C01B21/50; {compounds of noble gases C01B23/0005}; phosphides C01B25/08; salts of oxyacids of phosphorus C01B25/16; carbides C01B32/90; compounds containing silicon C01B33/00; compounds containing boron C01B35/00; compounds having molecular sieve properties but not having base-exchange properties C01B37/00; compounds having molecular sieve and base-exchange properties, e.g. crystalline zeolites, C01B39/00; cyanides C01C3/08; salts of cyanamide C01C3/16; thiocyanates C01C3/20)
- C01P: INDEXING SCHEME RELATING TO STRUCTURAL AND PHYSICAL ASPECTS OF SOLID INORGANIC COMPOUNDS
- Y02E: REDUCTION OF GREENHOUSE GAS [GHG] EMISSIONS, RELATED TO ENERGY GENERATION, TRANSMISSION OR DISTRIBUTION

## Abstract

The present disclosure relates to a positive electrode active material including: a lithium nickel-based transition metal oxide with a large particle diameter and a lithium nickel-based transition metal oxide with a small particle diameter. The lithium nickel-based transition metal oxide with a large particle diameter is a secondary particle. The lithium nickel-based transition metal oxide with a small particle diameter is a single particle formed of one nodule and/or a quasi-single particle that is a composite of 30 or less nodules. The lithium nickel-based transition metal oxide with a large particle diameter has a D50 of 5 μm to 30 μm, a Z value defined by factors of roundness distribution characteristics of 1.0 to 9.0, and a negative skewness factor (NSF) of 0.1 to 0.9. Use of the positive electrode active material in a lithium secondary battery results in improved lifespan and/or output characteristics of the battery.

## Claims

### Claim 1

A positive electrode active material comprising:
a lithium nickel-based transition metal oxide with a large particle diameter and a lithium nickel-based transition metal oxide with a small particle diameter,
wherein the lithium nickel-based transition metal oxide with a large particle diameter is in the form of a secondary particle that is an aggregate of primary particles,
wherein the lithium nickel-based transition metal oxide with a small particle diameter is in the form of at least one of a single particle formed of one nodule and a quasi-single particle that is a composite of 30 or less nodules,
wherein the lithium nickel-based transition metal oxide with a large particle diameter has a D50 of from 5 μm to 30 μm, a
Z value defined by Equation 1 below that is from 1.0 to 9.0, and
a negative skewness factor (NSF) defined by Equation 2 below that is from 0.1 to 0.9:
Z
=
F
max
R
/
S
R
[
Equation
⁢
1
]
wherein the FRmax and SR− are values obtained when drawing a histogram with the number of particles as a frequency by dividing the degree of roundness into 0.05 units in a roundness dispersion obtained from a scanning electron microscope (SEM) and an image analysis program for the lithium nickel-based transition metal oxide with a large particle diameter, wherein the FRmax is the maximum frequency roundness ratio (mode roundness ratio), which is the frequency of the class (roundness) with the highest frequency (number of particles) divided by the total number of analyzed particles, and SR is the standard deviation of the roundness,
NSF
=
(
R
5
⁢
0
-
R
1
⁢
0
)
/
F
max
R
[
Equation
⁢
2
]
wherein the FRmax, R50 and R10− are values obtained when drawing a histogram with the number of particles as a frequency by dividing the degree of roundness into 0.05 units in a roundness dispersion obtained from a scanning electron microscope (SEM) and an image analysis program for the lithium nickel-based transition metal oxide with a large particle diameter, wherein the FRmax is the maximum frequency roundness ratio (mode roundness ratio), which is the frequency of the class (roundness) with the highest frequency (number of particles) divided by the total number of analyzed particles, R50 is a roundness at a point with a cumulative frequency of 50%, and R10 is a roundness at a point with a cumulative frequency of 10%.

### Claim 2 (depends on 1)

The positive electrode active material according to claim 1, wherein the Z value is 2.0 to 7.0.

### Claim 3 (depends on 1)

The positive electrode active material according to claim 1, wherein the negative skewness factor (NSF) is 0.2 to 0.7

### Claim 4 (depends on 1)

The positive electrode active material according to claim 1, wherein the standard deviation (SR) of the roundness is 0.05 to 0.15.

### Claim 5 (depends on 1)

The positive electrode active material according to claim 1, wherein the maximum frequency roundness ratio (FRmax) is 0.1 to 0.4.

### Claim 6 (depends on 1)

The positive electrode active material according to claim 1, wherein the mixed weight ratio of the large-particle-diameter lithium nickel-based transition metal oxide to the small-particle-diameter lithium nickel-based transition metal oxide is 9:1 to 3:7.

### Claim 7 (depends on 1)

The positive electrode active material according to claim 1, wherein the positive electrode active material has an aspect ratio of 0.60 to 0.99, and a roundness of 0.60 to 0.99.

### Claim 8 (depends on 1)

The positive electrode active material according to claim 1, wherein each of the lithium nickel-based transition metal oxide with a large particle diameter and the lithium nickel-based transition metal oxide with a small particle diameter is independently represented by the following chemical formula (1):
wherein M1 includes one or more selected from Mn or Al; M2 includes one or more selected from the group consisting of W, Zr, Y, Ba, Ca, Ti, V, Mg, Ta or Nb; X includes one or more selected from the group consisting of N, P, S, F or Cl; and 0≤x≤0.5, 0.5≤a<1, 0<b≤0.4, 0<c≤0.4, 0≤d≤0.05, and 0≤e≤0.05.

### Claim 9 (depends on 1)

The positive electrode active material according to claim 1, wherein each of the lithium nickel-based transition metal oxide with a large particle diameter and the lithium nickel-based transition metal oxide with a small particle diameter independently have a nickel content in the lithium nickel-based transition metal oxide of 70 mol % or more.

### Claim 10 (depends on 1)

A positive electrode comprising the positive electrode active material according to claim 1.

### Claim 11 (depends on 10)

A lithium secondary battery comprising the positive electrode of claim 10.

### Claim 12 (depends on 1)

The positive electrode active material according to claim 1, wherein the lithium nickel-based transition metal oxide with a small particle diameter is in the form of a single particle formed of one nodule.

### Claim 13 (depends on 1)

The positive electrode active material according to claim 1, wherein the lithium nickel-based transition metal oxide with a small particle diameter is in the form of
a quasi-single particle that is a composite of 30 or less nodules.

### Claim 14 (depends on 1)

The positive electrode active material of claim 1, wherein the lithium nickel-based transition metal oxide with a large particle diameter has a D50 of 10 μm to 30 μm.

### Claim 15 (depends on 1)

The positive electrode active material of claim 1, wherein the positive electrode active material has a bimodal particle size distribution.

### Claim 16 (depends on 1)

The positive electrode active material of claim 1, wherein the Z value is 2.0 to 7.0 and the negative skewness factor (NSF) is 0.2 to 0.7.

### Claim 17 (depends on 8)

The positive electrode active material of claim 8, wherein M1 includes Mn.

### Claim 18 (depends on 8)

The positive electrode active material of claim 8, wherein M1 includes Mn and Al.

### Claim 19 (depends on 8)

The positive electrode active material of claim 8, wherein M2 includes one or more selected from the group consisting of Zr, Y, Mg, or Ti.

### Claim 20 (depends on 9)

The positive electrode active material of claim 9, wherein each of the lithium nickel-based transition metal oxide with a large particle diameter and the lithium nickel-based transition metal oxide with a small particle diameter independently have a nickel content in the lithium nickel-based transition metal oxide of 75 mol % or more.