# US 2026/0071292 A1 · Hot rolled and heat-treated steel sheet and method of manufacturing the same

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2026/0071292 A1
- Document ID: US20260071292A1
- Status: Published application
- Kind: A1
- Application number: 19/395,763
- Filed: 2025-11-20
- Published: 2026-03-12
- Earliest claimed: 2019-12-19
- Applicants: ArcelorMittal
- Inventors: Astrid PERLADE; Kangying ZHU; Coralie JUNG; Frédéric KEGEL
- Web page: https://patentgrep.com/patent/US20260071292A1

## CPC

- C21D 9/46: for sheet metals
- B21B 1/22: for rolling {plates, strips,} bands or sheets of indefinite length (B21B1/42 takes precedence)
- C21D 1/18: Hardening (C21D1/02 takes precedence); Quenching with or without subsequent tempering (quenching devices C21D1/62)
- C21D 1/26: Methods of annealing
- C21D 6/005: {containing Mn}
- C21D 6/008: {containing Si}
- C21D 8/02: during manufacturing of plates or strips (C21D8/12 takes precedence)
- C21D 8/0226: {Hot rolling}
- C21D 8/0263: {following hot rolling}
- C22C 38/001: {containing N}
- C22C 38/002: {containing In, Mg, or other elements not provided for in one single group C22C38/001 - C22C38/60}
- C22C 38/02: containing silicon
- C22C 38/04: containing manganese
- C22C 38/06: containing aluminium
- C22C 38/12: containing tungsten, tantalum, molybdenum, vanadium, or niobium
- C22C 38/14: containing titanium or zirconium
- B21B 2001/225: {by hot-rolling}
- C21D 2211/001: Austenite
- C21D 2211/002: Bainite
- C21D 2211/004: Dispersions; Precipitations
- C21D 2211/005: Ferrite
- C21D 2211/008: Martensite
- C21D: MODIFYING THE PHYSICAL STRUCTURE OF FERROUS METALS; GENERAL DEVICES FOR HEAT TREATMENT OF FERROUS OR NON-FERROUS METALS OR ALLOYS; MAKING METAL MALLEABLE, e.g. BY DECARBURISATION OR TEMPERING (surface treatment of metallic material involving at least one process provided for in class C23 and at least one process covered by this subclass C23F17/00; unidirectional solidification of eutectic materials or unidirectional demixing of eutectoid materials C30B)
- B21B: ROLLING OF METAL (auxiliary operations used in connection with metal-working operations covered in B21, see B21C; bending by rolling B21D; manufacture of particular objects, e.g. screws, wheels, rings, barrels, balls, by rolling B21H; pressure welding by means of a rolling mill B23K20/04)
- C22C: ALLOYS (treatment of alloys C21D, C22F)

## Abstract

A method for manufacturing a hot rolled and heat-treated steel sheet includes casting to obtain a semi-finished product having a composition comprising, by weight percent: C: 0.12-0.25%, Mn: 3.0-8.0%, Si: 0.7-1.5%, Al: 0.3-1.2%, B: 0.0002-0.004%, S≤0.010%, P≤0.020%, N≤0.008%, and iron; reheating at a Treheat between 1150° C. and 1300° C.; hot rolling the reheated semi-finished product with a finish rolling temperature (Tnr-100° C. to 950° C.), coiling the hot rolled steel sheet at a Tcoil (20° C. and 700° C.) and cooling to obtain a microstructure comprising martensite and bainite, M+B>80%, F<20%, and <20% of the sum of martensite-austenite (M-A) islands and carbides, and having the multiplication of PAGS <1000 μm2 and a pancaking index <5; reheating, quenching, reheating to a partitioning temperature, holding for 1 to 1000 seconds, and cooling.

## Claims

### Claim 1

A method for manufacturing a hot rolled and heat-treated steel sheet, comprising the following successive steps:
casting a steel to obtain a semi-finished product, said semi-finished product having a composition comprising, by weight percent:
C: 0.12-0.25%
Mn: 3.0-8.0%
Si: 0.7-1.5%
Al: 0.3-1.2%
B: 0.0002-0.004%
S≤0.010%
P≤0.020%
N≤0.008%
and optionally one or more of the following elements, in weight percentage:
Mo≤0.5%
V≤0.2%
Nb≤0.06%
Ti≤0.05%
a remainder of the composition being iron and unavoidable impurities resulting from processing;
reheating the semi-finished product at a temperature Treheat between 1150° C. and 1300° C.;
hot rolling the reheated semi-finished product with a finish rolling temperature FRT between Tnr-100° C. and 950° C. to obtain a hot rolled steel sheet, Tnr being the non-recrystallisation temperature defined as
825
+
2300
⋆
%
⁢
Nb
+
710
⋆
%
⁢
Ti
+
150
⋆
%
⁢
Mo
+
120
⋆
%
⁢
V
+
8
⋆
%
⁢
Mn
;
coiling the hot rolled steel sheet at a coiling temperature Tcoil comprised between 20° C. and 700° C. and cooling to room temperature so to obtain, a microstructure comprising martensite and bainite, the sum of which being greater than 80%, strictly less than 20% of ferrite, and strictly less than 20% of the sum of martensite-austenite (M-A) islands and carbides, and having the multiplication of PAGS in rolling direction by PAGS in normal direction lower than 1000 μm2 and a pancaking index lower than 5;
reheating the hot rolled steel sheet to a temperature TA1 strictly lower than Ae3 and higher than (Ae1+Ae3)/2, and maintaining the steel sheet at the annealing temperature TA1 for a holding time tA1 between 3 s and 1000 s, Ae1 and Ae3 temperature being defined as
Ae
⁢
1
=
670
+
15
⋆
%
⁢
Si
-
13
⋆
%
⁢
Mn
+
18
⋆
%
⁢
Al
Ae
⁢
3
=
890
-
20
⋆
√
%
⁢
C
+
20
⋆
%
⁢
Si
-
30
⋆
%
⁢
Mn
+
130
*
%
⁢
Al
quenching the hot-rolled steel sheet to a quenching temperature TQ lower than (Ms-50° C.), to obtain a quenched steel sheet, Ms being defined as
Ms
=
560
-
(
30
*
%
⁢
Mn
+
13
⋆
%
⁢
Si
-
15
⋆
%
⁢
Al
+
12
⋆
%
⁢
Mo
)
-
600
⋆
(
1
-
exp
(
-
0
,
96
⋆
%
⁢
C
)
)
;
reheating the quenched steel sheet to a partitioning temperature TP comprised between 350° C. and 550° C., and maintaining the quenched steel sheet at the partitioning temperature for a partitioning time between 1 s and 1000 s; and
cooling the steel sheet to the room temperature to obtain a hot rolled and heat-treated steel sheet.

### Claim 2 (depends on 1)

The method as recited in claim 1 wherein the manganese content is comprised between 3.0% and 5.0%, by weight.

### Claim 3 (depends on 1)

The method as recited in claim 1 wherein the silicon content is comprised between 0.8% and 1.3%, by weight.

### Claim 4 (depends on 1)

The method as recited in claim 1 wherein a yield strength of the hot rolled and heat-treated steel sheet is higher than 950 MPa.

### Claim 5 (depends on 1)

The method as recited in claim 1 wherein a tensile strength of the hot rolled and heat-treated steel sheet is higher than 1180 MPa.

### Claim 6 (depends on 1)

The method as recited in claim 1 wherein a uniform elongation of the hot rolled and heat-treated steel sheet is higher than 10%.

### Claim 7 (depends on 1)

The method as recited in claim 1 wherein a hole expansion ratio of the hot rolled and heat-treated steel sheet is higher than 25%.

### Claim 8 (depends on 1)

The method as recited in claim 1, wherein the hot rolled and heat-treated steel sheet has a microstructure consisting of, in surface fraction: between 5% and 45% of ferrite; between 25% and 85% of partitioned martensite, the partitioned martensite having a carbide density less than 2×106/mm2; between 10% and 30% of retained austenite; less than 8% of fresh martensite, a part of said fresh martensite being combined with retained austenite in the shape of martensite-austenite (M-A) islands in total surface fraction less than 10%; and a pancaking index lower than 5.

### Claim 9 (depends on 8)

The method as recited in claim 8 wherein fresh martensite and martensite-austenite islands size of the hot rolled and heat-treated steel sheet are less than 0.7 μm.

### Claim 10 (depends on 8)

The method as recited in claim 8 wherein the microstructure of the hot rolled and heat-treated steel sheet includes the fresh martensite and the M-A islands.

### Claim 11 (depends on 8)

The method as recited in claim 8 wherein the M-A islands of the hot rolled and heat-treated steel sheet have an aspect ratio lower or equal to 2.

### Claim 12 (depends on 8)

The method as recited in claim 8 wherein the fresh martensite conent of the hot rolled and heat-treated steel sheet is 2% to less than 8%.

### Claim 13 (depends on 8)