# US 2026/0066341 A1 · Solid electrolyte, method of preparing the same, and all-solid-state battery including the solid electrolyte

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2026/0066341 A1
- Document ID: US20260066341A1
- Status: Published application
- Kind: A1
- Application number: 19/105,257
- Filed: 2023-10-31
- Published: 2026-03-05
- Earliest claimed: 2022-10-31
- Assignees: LG Chem, Ltd.; Iucf-Hyu (Industry-University Cooperation Foundation Hanyang University)
- Applicants: LG Chem, Ltd.; Iucf-Hyu (Industry-University Cooperation Foundation Hanyang University)
- Inventors: Seong Ho LEE; Tae Seup SONG; Jeong Heon KIM; Seung Woo LEE; Chang Hun PARK; Sang Hyuk MIN; Byoung Kuk SON
- Web page: https://patentgrep.com/patent/US20260066341A1

## CPC

- H01M 10/0562: Solid materials
- C01B 25/14: Sulfur, selenium, or tellurium compounds of phosphorus
- C01D 15/00: Lithium compounds
- H01M 10/052: Li-accumulators
- C01P 2004/61: Micrometer sized, i.e. from 1-100 micrometer
- C01P 2004/84: one phase coated with the other
- H01M 2300/0068: inorganic
- H01M 2300/008: Halides
- H01M 2300/0094: in the form of layered products, e.g. coatings
- Y02E 60/10: Energy storage using batteries
- H01M: PROCESSES OR MEANS, e.g. BATTERIES, FOR THE DIRECT CONVERSION OF CHEMICAL ENERGY INTO ELECTRICAL ENERGY
- C01B: NON-METALLIC ELEMENTS; COMPOUNDS THEREOF; {METALLOIDS OR COMPOUNDS THEREOF NOT COVERED BY SUBCLASS C01C}
- C01D: COMPOUNDS OF ALKALI METALS, i.e. LITHIUM, SODIUM, POTASSIUM, RUBIDIUM, CAESIUM, OR FRANCIUM (metal hydrides {monoborane, diborane or addition complexes thereof} C01B6/00; salts of oxyacids of halogens C01B11/00; peroxides, salts of peroxyacids C01B15/00; sulfides C01B17/22; thiosulfates, dithionites, polythionates C01B17/64; compounds containing selenium or tellurium C01B19/00; binary compounds of nitrogen with metals C01B21/06; azides C01B21/08; {compounds other than ammonia and cyanogen, containing nitrogen and other non-metals C01B21/082}; metal amides C01B21/092; nitrites C01B21/50; phosphides C01B21/50; {compounds of noble gases C01B23/0005}; phosphides C01B25/08; salts of oxyacids of phosphorus C01B25/16; carbides C01B32/90; compounds containing silicon C01B33/00; compounds containing boron C01B35/00; cyanides C01C3/08; salts of cyanic acid C01C3/14; salts of cyanamide C01C3/16; thiocyanates C01C3/20)
- C01P: INDEXING SCHEME RELATING TO STRUCTURAL AND PHYSICAL ASPECTS OF SOLID INORGANIC COMPOUNDS
- Y02E: REDUCTION OF GREENHOUSE GAS [GHG] EMISSIONS, RELATED TO ENERGY GENERATION, TRANSMISSION OR DISTRIBUTION

## Abstract

The present invention relates to a sulfide-based solid electrolyte having excellent moisture stability and ionic conductivity, a method of preparing the same, and an all-solid-state battery including the sulfide-based solid electrolyte, wherein the present invention provides a solid electrolyte which includes a core portion including sulfide-based solid electrolyte particles; and a surface portion which is formed on the core portion and includes fluorine-doped sulfide-based solid electrolyte particles, wherein the surface portion includes a concentration gradient region in which a concentration of a fluorine (F) atom is decreased from a surface of the surface portion toward the core portion, a method of preparing the same, and an all-solid-state battery including the solid electrolyte.

## Claims

### Claim 1

A solid electrolyte comprising:
a core portion including sulfide-based solid electrolyte particles; and
a surface portion that is formed on the core portion and includes fluorine-doped sulfide-based solid electrolyte particles,
wherein the surface portion comprises a concentration gradient region in which a concentration of a fluorine (F) atom is decreased from a surface of the surface portion toward the core portion.

### Claim 2 (depends on 1)

The solid electrolyte of claim 1, wherein the fluorine-doped sulfide-based solid electrolyte particles are represented by Formula 1:
wherein, in Formula 1,
B is phosphorus (P), arsenic (As), germanium (Ge), gallium (Ga), antimony (Sb), silicon (Si), tin (Sn), aluminum (Al), indium (In), titanium (Ti), vanadium (V), niobium (Nb), or tantalum (Ta),
X is selenium (Se) or tellurium (Te),
Y is chlorine (Cl), bromine (Br), iodine (I), CN, OCN, SCN, or N3, and
x satisfies 0≤x≤2, a satisfies 0≤a≤2, and b satisfies 0.1<b≤1.0.

### Claim 3 (depends on 1)

The solid electrolyte of claim 1, wherein the fluorine-doped sulfide-based solid electrolyte particles are represented by Formula 1-1:
wherein, in Formula 1-1,
b satisfies 0.1<b≤1.0.

### Claim 4 (depends on 1)

The solid electrolyte of claim 1, wherein the sulfide-based solid electrolyte particles are an argyrodite-type solid electrolyte.

### Claim 5 (depends on 1)

The solid electrolyte of claim 1, wherein the sulfide-based solid electrolyte particles are represented by Formula 2:
wherein, in Formula 2,
B is P, As, Ge, Ga, Sb, Si, Sn, Al, In, Ti, V, Nb, or Ta,
X is Se or Te,
Y is Cl, Br, I, CN, OCN, SCN, or N3, and
x satisfies 0≤x≤2, and a satisfies 0≤a≤2.

### Claim 6 (depends on 1)

The solid electrolyte of claim 1, wherein the concentration gradient region comprises a region from a surface of the solid electrolyte to a distance of 30 nm or more to less than 1,200 nm toward a center.

### Claim 7 (depends on 1)

The solid electrolyte of claim 1, wherein an average particle diameter is in a range of 2 μm to 10 μm.

### Claim 8

A method of preparing a solid electrolyte, the method comprising a step of heat-treating sulfide-based solid electrolyte particles in the presence of ammonium fluoride in an inert gas atmosphere,
wherein the ammonium fluoride is used in an amount of 1 part by weight to 10 parts by weight based on 100 parts by weight of the sulfide-based solid electrolyte particles.

### Claim 9 (depends on 8)

The method of claim 8, wherein the sulfide-based solid electrolyte particles are an argyrodite-type solid electrolyte.

### Claim 10 (depends on 8)

The method of claim 8, wherein the heat-treating is performed by sequentially performing a first heat treatment step and a second heat treatment step,
wherein the first heat treatment step is performed at a temperature of 200° C. to 300° C. for 1 hour to 5 hours, and
the second heat treatment step is performed at a temperature of 400° C. to 600° C. for 5 hours to 10 hours.

### Claim 11 (depends on 1)

An all-solid-state battery comprising:
a positive electrode;
a negative electrode; and
the solid electrolyte of claim 1.