# US 2026/0066296 A1 · Anode active material, manufacturing method thereof, anode and secondary battery including the same

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2026/0066296 A1
- Document ID: US20260066296A1
- Status: Published application
- Kind: A1
- Application number: 19/379,992
- Filed: 2025-11-05
- Published: 2026-03-05
- Earliest claimed: 2021-07-02
- Assignees: Industry-Academic Cooperation Foundation, Dankook University
- Applicants: Industry-Academic Cooperation Foundation, Dankook University
- Inventors: Byoungsun LEE
- Web page: https://patentgrep.com/patent/US20260066296A1

## CPC

- H01M 4/587: for inserting or intercalating light metals
- C01B 32/05: Preparation or purification of carbon not covered by groups C01B32/15, C01B32/20, C01B32/25, C01B32/30
- C01B 32/205: Preparation
- C01B 32/21: After-treatment
- H01M 4/133: Electrodes based on carbonaceous material, e.g. graphite-intercalation compounds or CFx
- H01M 4/1393: of electrodes based on carbonaceous material, e.g. graphite-intercalation compounds or CFx
- H01M 4/36: Selection of substances as active materials, active masses, active liquids
- H01M 4/364: {as mixtures}
- H01M 4/625: {Carbon or graphite}
- H01M 10/052: Li-accumulators
- H01M 10/0525: Rocking-chair batteries, i.e. batteries with lithium insertion or intercalation in both electrodes; Lithium-ion batteries
- H01M 10/054: Accumulators with insertion or intercalation of metals other than lithium, e.g. with magnesium or aluminium
- C01P 2004/03: obtained by SEM
- C01P 2004/32: Spheres
- C01P 2004/50: Agglomerated particles
- C01P 2004/51: Particles with a specific particle size distribution
- C01P 2004/52: highly monodisperse size distribution
- C01P 2004/60: Particles characterised by their size
- C01P 2004/61: Micrometer sized, i.e. from 1-100 micrometer
- C01P 2004/62: Submicrometer sized, i.e. from 0.1-1 micrometer
- C01P 2004/64: Nanometer sized, i.e. from 1-100 nanometer
- C01P 2006/12: Surface area
- C01P 2006/40: Electric properties
- H01M 2004/021: {Physical characteristics, e.g. porosity, surface area}
- H01M 2004/027: {Negative electrodes}
- Y02E 60/10: Energy storage using batteries
- H01M: PROCESSES OR MEANS, e.g. BATTERIES, FOR THE DIRECT CONVERSION OF CHEMICAL ENERGY INTO ELECTRICAL ENERGY
- C01B: NON-METALLIC ELEMENTS; COMPOUNDS THEREOF; {METALLOIDS OR COMPOUNDS THEREOF NOT COVERED BY SUBCLASS C01C}
- C01P: INDEXING SCHEME RELATING TO STRUCTURAL AND PHYSICAL ASPECTS OF SOLID INORGANIC COMPOUNDS
- Y02E: REDUCTION OF GREENHOUSE GAS [GHG] EMISSIONS, RELATED TO ENERGY GENERATION, TRANSMISSION OR DISTRIBUTION

## Abstract

The present invention relates to an anode active material, a method of manufacturing the anode active material, and an anode and a secondary battery including the anode active material, the anode active material including secondary carbon particles formed by flocculation of a plurality of primary carbon particles having an average particle diameter (D50) in a range from 5 to 200 nm, wherein the secondary carbon particles have an average particle diameter (D50) in a range from 0.5 to 20 μm.

## Claims

### Claim 1

An anode active material for a secondary battery comprising:
secondary carbon particles formed by flocculation of a plurality of primary carbon particles having an average particle diameter (D50) in a range from 5 to 200 nm,
wherein the secondary carbon particles have an average particle diameter (D50) in a range from 0.5 to 20 μm, a specific surface area in a range from 0.5 to 100 m2/g, and a spherical porous structure.

### Claim 2 (depends on 1)

The anode active material of claim 1, wherein the secondary carbon particles have a particle size distribution that satisfies the following Relational Expression 1:
0.4
≤
(
D
9
⁢
0
-
D
10
)
/
D
5
⁢
0
≤
0.7
,
[
Relational
⁢
Expression
⁢
1
]
(in the above Relational Expression 1,
D90, D10 and D50 are particle sizes having a cumulative volume of 90% by volume, a particle size having a cumulative volume of 10% by volume, and a particle size having a cumulative volume of 50% by volume, respectively, in a volume-based particle size distribution by a laser diffraction particle size distribution measuring method.)

### Claim 3 (depends on 1)

The anode active material of claim 1, further comprising graphite.

### Claim 4 (depends on 3)

The anode active material of claim 3, wherein a ratio (D2/D1) of a particle diameter (D2) of the graphite to a particle diameter (D1) of the secondary carbon particle is in a range from 2 to 8, and
the secondary carbon particles and graphite are included in a ratio in a range from 5:95 to 90:10 by weight.

### Claim 5 (depends on 1)

An anode for a secondary battery comprising the anode active material of claim 1, wherein the anode active material comprises:
secondary carbon particles formed by flocculation of a plurality of primary carbon particles having an average particle diameter (D50) in a range from 5 to 200 nm,
wherein the secondary carbon particles have an average particle diameter (D50) in a range from 0.5 to 20 μm, a specific surface area in a range from 0.5 to 100 m2/g, and a spherical porous structure.

### Claim 6

A method of manufacturing an anode active material for a secondary battery, the method comprising:
(S100) forming a first solution by dissolving a carbonization precursor polymer and a sacrificial polymer in a first solvent which is a common solvent;
(S200) forming a first aggregate by removing the first solvent from the first solution; and
(S300) carbonizing the first aggregate, or carbonizing a second aggregate formed by removing the sacrificial polymer from the first aggregate.

### Claim 7 (depends on 6)

The method of claim 6, wherein the second aggregate is formed by:
forming a second solution including the second aggregate by dissolving the sacrificial polymer in the first aggregate with a second solvent for dissolving the sacrificial polymer; and
separating the second aggregate from the second solution.

### Claim 8 (depends on 6)

The method of claim 6, wherein the carbonization precursor polymer and the sacrificial polymer are used in a ratio in a range from 1:2 to 9 by weight.

### Claim 9 (depends on 6)

The method of claim 6, wherein the carbonization precursor polymer comprises one or more of: polyacrylonitrile (PAN), polyvinyl pyrrolidine (PVP), polyimide, polyvinyl alcohol (PVA), polyvinyl chloride (PVC), pitch, lignin and cellulose.

### Claim 10 (depends on 6)

The method of claim 6, wherein the sacrificial polymer comprises one or more of: styrene-co-acrylonitrile (SAN), polylactic acid (PLA), poly(lactic-co-glycolic acid) (PLGA), polymethacrylate (PMMA), and poly(vinylidene fluoride) (PVDF).

### Claim 11 (depends on 6)

The method of claim 6, further comprising a metal precursor including one or more metal M of a group 13 element, a group 14 element and a transition metal in the first solvent.

### Claim 12 (depends on 11)

The method of claim 11, wherein the metal precursor is added so that an element ratio of C:M is in a range from 10 to 1:1 with respect to carbon (C) in the carbonization precursor polymer.

### Claim 13 (depends on 7)

The method of claim 7, wherein a ratio (W2/W1) of a content (W2) of the second solvent to a content (W1) of the sacrificial polymer is in a range from 18 to 22.

### Claim 14 (depends on 7)

The method of claim 7, wherein the first aggregate and the second solvent are used in a ratio in a range from 1:14 to 18 by weight.

### Claim 15 (depends on 6)

The method of claim 6, wherein in the carbonizing, the first aggregate or the second aggregate is heat-treated after raising a temperature to a range from 600 to 1600° C. in an inert gas atmosphere.

### Claim 16 (depends on 15)

The method of claim 15, wherein the carbonizing is performed after raising a temperature to a range from 200 to 300° C. and then stabilizing the first aggregate or the second aggregate in an oxygen-containing atmosphere by heat-treating.