# US 2026/0062765 A1 · High-strength coated steel sheet and method for producing the same

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2026/0062765 A1
- Document ID: US20260062765A1
- Status: Published application
- Kind: A1
- Application number: 19/120,851
- Filed: 2023-08-31
- Published: 2026-03-05
- Earliest claimed: 2022-10-27
- Assignees: Jfe Steel Corporation
- Applicants: JFE Steel Corporation
- Inventors: Kazuki ENDOH; Yoshiyasu KAWASAKI; Yuki TOJI; Masaki TADA; Katsutoshi TAKASHIMA
- Web page: https://patentgrep.com/patent/US20260062765A1

## CPC

- C21D 9/46: for sheet metals
- B32B 15/013: {one layer being formed of an iron alloy or steel, another layer being formed of a metal other than iron or aluminium}
- C21D 1/185: {from an intercritical temperature}
- C21D 1/19: by interrupted quenching
- C21D 1/25: Hardening, combined with annealing between 300 degrees Celsius and 600 degrees Celsius, i.e. heat refining ("Vergüten")
- C21D 1/26: Methods of annealing
- C21D 6/001: {containing Ni (C21D6/004 takes precedence)}
- C21D 6/002: {containing Cr (C21D6/004 takes precedence)}
- C21D 6/005: {containing Mn}
- C21D 6/007: {containing Co}
- C21D 6/008: {containing Si}
- C21D 8/02: during manufacturing of plates or strips (C21D8/12 takes precedence)
- C21D 8/0226: {Hot rolling}
- C21D 8/0236: {Cold rolling}
- C21D 8/0263: {following hot rolling}
- C21D 8/0273: {Final recrystallisation annealing}
- C21D 8/0278: involving a particular surface treatment (C21D8/0294 takes precedence)
- C22C 38/001: {containing N}
- C22C 38/002: {containing In, Mg, or other elements not provided for in one single group C22C38/001 - C22C38/60}
- C22C 38/005: {containing rare earths, i.e. Sc, Y, Lanthanides}
- C22C 38/008: {containing tin}
- C22C 38/02: containing silicon
- C22C 38/04: containing manganese
- C22C 38/06: containing aluminium
- C22C 38/08: containing nickel {(C22C38/105 takes precedence)}
- C22C 38/10: containing cobalt
- C22C 38/12: containing tungsten, tantalum, molybdenum, vanadium, or niobium
- C22C 38/14: containing titanium or zirconium
- C22C 38/16: containing copper
- C22C 38/28: with titanium or zirconium
- C22C 38/34: with more than 1.5% by weight of silicon
- C22C 38/38: with more than 1.5% by weight of manganese
- C22C 38/50: with titanium or zirconium
- C22C 38/58: with more than 1.5% by weight of manganese
- C22C 38/60: containing lead, selenium, tellurium, or antimony, or more than 0.04% by weight of sulfur
- C23C 2/0224: {Two or more thermal pretreatments}
- C23C 2/06: Zinc or cadmium or alloys based thereon
- C23C 2/28: Thermal after-treatment, e.g. treatment in oil bath
- C23C 2/40: Plates; Strips
- B32B 2311/20: Zinc
- B32B 2311/30: Iron, e.g. steel
- C21D 2211/001: Austenite
- C21D 2211/002: Bainite
- C21D 2211/005: Ferrite
- C21D 2211/008: Martensite
- C21D: MODIFYING THE PHYSICAL STRUCTURE OF FERROUS METALS; GENERAL DEVICES FOR HEAT TREATMENT OF FERROUS OR NON-FERROUS METALS OR ALLOYS; MAKING METAL MALLEABLE, e.g. BY DECARBURISATION OR TEMPERING (surface treatment of metallic material involving at least one process provided for in class C23 and at least one process covered by this subclass C23F17/00; unidirectional solidification of eutectic materials or unidirectional demixing of eutectoid materials C30B)
- B32B: LAYERED PRODUCTS, i.e. PRODUCTS BUILT-UP OF STRATA OF FLAT OR NON-FLAT, e.g. CELLULAR OR HONEYCOMB, FORM
- C22C: ALLOYS (treatment of alloys C21D, C22F)
- C23C: COATING METALLIC MATERIAL; COATING MATERIAL WITH METALLIC MATERIAL; SURFACE TREATMENT OF METALLIC MATERIAL BY DIFFUSION INTO THE SURFACE, BY CHEMICAL CONVERSION OR SUBSTITUTION; COATING BY VACUUM EVAPORATION, BY SPUTTERING, BY ION IMPLANTATION OR BY CHEMICAL VAPOUR DEPOSITION, IN GENERAL (making metal-coated products by extrusion B21C23/22; covering with metal by connecting pre-existing layers to articles, see the relevant places, e.g. B21D39/00, B23K; metallising of glass C03C; metallising mortars, concrete, artificial stone, ceramics or natural stone C04B41/00; enamelling of, or applying a vitreous layer to, metals C23D; treating metal surfaces or coating of metals by electrolysis or electrophoresis C25D; single-crystal film growth C30B; by metallising textiles D06M11/83; decorating textiles by locally metallising D06Q1/04)

## Abstract

A high-strength coated steel sheet having a TS of 1180 MPa or more and a method for producing the high-strength coated steel sheet are disclosed. The high-strength coated steel sheet has a prescribed chemical composition. The high-strength coated steel sheet has, at a position ¼ of the sheet thickness, a steel microstructure in which the area fraction of ferrite is 1% or more and 30% or less, in which the area fraction of fresh martensite is 1% or less and 15% or more, in which the total area fraction of bainite and tempered martensite is 35% or more and 90% or less, and in which the area fraction of retained austenite is 6% or more. A value obtained by dividing the average amount of Mn in retained austenite grains having an aspect ratio of 2.0 or more by the average amount of Mn in ferrite is 1.1 or more.

## Claims

### Claim at position 1

1-9. (canceled)

### Claim 10

A high-strength coated steel sheet having a chemical composition containing, in % by mass,
C: 0.030% or more and 0.300% or less,
Si: 0.01% or more and 2.50% or less,
Mn: 0.10% or more and 8.00% or less,
P: 0.100% or less,
S: 0.0200% or less,
Al: 0.100% or less,
N: 0.0100% or less, and
O: 0.0100% or less,
with the balance being Fe and incidental impurities,
wherein the high-strength coated steel sheet has, at a position ¼ of a sheet thickness,
a steel microstructure in which an area fraction of ferrite is 1% or more and 30% or less, in which an area fraction of fresh martensite is 1% or more and 15% or less, in which a total area fraction of bainite and tempered martensite is 35% or more and 90% or less, and in which an area fraction of retained austenite is 6% or more,
wherein a value obtained by dividing an average amount (% by mass) of Mn in retained austenite grains having an aspect ratio of 2.0 or more by an average amount (% by mass) of Mn in the ferrite is 1.1 or more,
wherein Mnγeq. determined from formula (1) is 5.0 or more, and
wherein δLME determined from formula (2) is 1.0 or less:
Mn
eq
.
γ
=
{
ln
⁡
(
[
C
]
⁢
γ
-
0.2
)
+
ln
⁡
(
[
Mn
]
⁢
γ
-
2.6
)
+
4.3
}
×
λγ
/
D
⁢
γ
,
(
1
)
δ
L
⁢
M
⁢
E
=
1
/
2
×
log
⁢
{
(
1
+
[
C
]
)
/
(
0.35
-
[
C
]
)
}
+
{
exp
⁡
(
[
Si
]
/
3.23
)
-
1
}
+
{
exp
⁡
(
[
Mn
]
/
22
)
-
1
}
(
2
)
where [C]γ and [Mn]γ are an average amount (% by mass) of C and an average amount (% by mass) of Mn, respectively, that are averaged over all retained austenite grains;
λγ is an average aspect ratio of all the retained austenite grains;
Dγ is an average equivalent circular diameter (μm) of all the retained austenite grains; and
[C], [Si], and [Mn] are an amount (% by mass) of C, an amount (% by mass) of Si, and an amount (% by mass) of Mn, respectively, with respect to a total amount of the steel sheet.

### Claim 11 (depends on 10)

The high-strength coated steel sheet according to claim 10, wherein the chemical composition further contains, in mass %, at least one element selected from
Ti: 0.200% or less, Nb: 0.200% or less,
V: 0.200% or less, Ta: 0.10% or less,
W: 0.10% or less, B: 0.0100% or less,
Cr: 1.00% or less, Mo: 1.00% or less,
Co: 1.000% or less, Ni: 1.00% or less,
Cu: 1.00% or less, Sn: 0.200% or less,
Sb: 0.200% or less, Ca: 0.0100% or less,
Mg: 0.0100% or less, REMs: 0.0100% or less,
Zr: 0.100% or less, Te: 0.100% or less,
Hf: 0.10% or less, and Bi: 0.200% or less.

### Claim 12 (depends on 10)

The high-strength coated steel sheet according to claim 10, wherein a value obtained by dividing a total amount of C in all the retained austenite grains by an amount of C in a T0 microstructure is less than 1.0.

### Claim 13 (depends on 11)

The high-strength coated steel sheet according to claim 11, wherein a value obtained by dividing a total amount of C in all the retained austenite grains by an amount of C in a T0 microstructure is less than 1.0.

### Claim 14 (depends on 10)

The high-strength coated steel sheet according to claim 10, wherein the high-strength coated steel sheet includes a galvanized layer.

### Claim 15 (depends on 11)

The high-strength coated steel sheet according to claim 11, wherein the high-strength coated steel sheet includes a galvanized layer.

### Claim 16 (depends on 12)

The high-strength coated steel sheet according to claim 12, wherein the high-strength coated steel sheet includes a galvanized layer.

### Claim 17 (depends on 13)

The high-strength coated steel sheet according to claim 13, wherein the high-strength coated steel sheet includes a galvanized layer.

### Claim 18 (depends on 14)

The high-strength coated steel sheet according to claim 14, wherein the galvanized layer is a galvannealed layer.

### Claim 19 (depends on 15)

The high-strength coated steel sheet according to claim 15, wherein the galvanized layer is a galvannealed layer.

### Claim 20 (depends on 16)

The high-strength coated steel sheet according to claim 16, wherein the galvanized layer is a galvannealed layer.

### Claim 21 (depends on 17)

The high-strength coated steel sheet according to claim 17, wherein the galvanized layer is a galvannealed layer.

### Claim 22 (depends on 10)

A method for producing the high-strength coated steel sheet according to claim 10, the method comprising:
heating a steel slab having the chemical composition;
hot-rolling at a finish rolling delivery temperature of 750° C. or higher and 1000° C. or lower;
coiling at 300° C. or higher and 750° C. or lower;
cold-rolling at a rolling reduction of 50% or less;
holding at a temperature in a range of higher than or equal to an Ac3 transformation temperature−50° C. for 20 s or longer and 1800 s or shorter; cooling to a cooling stop temperature lower than or equal to martensite start temperature;
reheating to a reheating temperature in a range of higher than or equal to Bs−150° C. and lower than or equal to Bs+150° C., where Bs is a temperature determined from formula (3); then holding at the reheating temperature for 2 s or longer and 1800 s or shorter; cooling to room temperature;
then heating to a temperature in a range from an Ac1 transformation temperature−150° C. to the Ac1 transformation temperature at a heating rate of 2° C./s or more; holding at a temperature in a range of higher than or equal to the Ac1 transformation temperature for 20 s or longer and 600 s or shorter; cooling to a cooling stop temperature lower than or equal to Ms′ determined from formula (4);
reheating to a reheating temperature in a range of higher than or equal to Ms′ and lower than or equal to Ms′+350° C.; holding at the reheating temperature for 2 s or longer and 600 s or shorter; performing coating treatment; and cooling to room temperature:
Bs
=
732
-
202
×
[
C
]
-
108
×
[
Si
]
-
85
×
[
Mn
]
-
39
×
[
Mo
]
,
(
3
)
where [C], [Si], [Mn], and [Mo] are an amount (% by mass) of C, an amount (% by mass) of Si, an amount (% by mass) of Mn, and an amount (% by mass) of Mo, respectively, with respect to the total amount of the steel sheet and are each zero when a corresponding element is not contained, and
Ms
′
=
Ms
×
15
/
Mn
eq
.
γ
,
(
4
)
where Ms is the martensite start temperature, and Mnγeq.=15 when Mnγeq.<15.

### Claim 23 (depends on 22)

The method for producing the high-strength coated steel sheet according to claim 22, wherein the coating treatment is galvanizing treatment.

### Claim 24 (depends on 23)

The method for producing the high-strength coated steel sheet according to claim 23, further comprising, after the galvanizing treatment, performing galvannealing treatment at 450° C. or higher and 600° C. or lower.

### Claim 25 (depends on 22)

The method for producing the high-strength coated steel sheet according to claim 22, further comprising, after the coiling but before the cold-rolling, holding at a temperature in a range of lower than or equal to the Ac1 transformation temperature for longer than 1800 s.