# US 2026/0061095 A1 · Bone collagen scaffold material loaded with multiple growth factors and a preparation method thereof

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2026/0061095 A1
- Document ID: US20260061095A1
- Status: Published application
- Kind: A1
- Application number: 19/283,269
- Filed: 2025-07-29
- Published: 2026-03-05
- Earliest claimed: 2024-08-28
- Assignees: Beijing Yiling Biotechnology Co., Ltd.; Xiling (Zhenjiang) Medical Science Co., Ltd.
- Applicants: Beijing Yiling Biotechnology Co., Ltd.; Xiling (Zhenjiang) Medical Science Co., Ltd.
- Inventors: Hui Sun; Lixin Xu; Manqi Yin; Wenhao Zhang; Feixiang Cai
- Web page: https://patentgrep.com/patent/US20260061095A1

## CPC

- A61L 27/24: Collagen
- A61L 27/3608: {Bone, e.g. demineralised bone matrix [DBM], bone powder}
- A61L 27/3687: {characterised by the use of chemical agents in the treatment, e.g. specific enzymes, detergents, capping agents, crosslinkers, anticalcification agents}
- A61L 27/54: Biologically active materials, e.g. therapeutic substances {(A61L27/227 takes precedence)}
- A61L 27/56: Porous materials, {e.g. foams or sponges}
- A61L 2300/414: Growth factors
- A61L 2430/02: for reconstruction of bones; weight-bearing implants
- A61L: METHODS OR APPARATUS FOR STERILISING MATERIALS OR OBJECTS IN GENERAL; DISINFECTION, STERILISATION OR DEODORISATION OF AIR; CHEMICAL ASPECTS OF BANDAGES, DRESSINGS, ABSORBENT PADS OR SURGICAL ARTICLES; MATERIALS FOR BANDAGES, DRESSINGS, ABSORBENT PADS OR SURGICAL ARTICLES (preservation of bodies or disinfecting characterised by the agents employed A01N; preserving, e.g. sterilising, food or foodstuffs A23; preparations for medical, dental or toiletry purposes A61K)

## Abstract

A bone collagen scaffold material loaded with multiple growth factors, which includes an acellular matrix for promoting growth of oral osteoblasts and multiple growth factors loaded on the acellular matrix; the acellular matrix is a bone collagen scaffold obtained from natural animal bone containing collagen; the multiple growth factors are FGF, VEGF, TGF-β, and BMP. The bone collagen scaffold material of the invention has a higher collagen content through secondary freeze-drying, making surface of the bone collagen scaffold material have a suitable pore size, guaranteeing mechanical properties and improve bone induction ability, being suitable for loading multiple growth factors and prolonging the degradation time to adapt to the therapeutic effect of periodontitis.

## Claims

### Claim 1

A bone collagen scaffold material loaded with multiple growth factors, wherein the bone collagen scaffold material includes an acellular matrix for promoting growth of oral osteoblasts and multiple growth factors loaded on the acellular matrix;
the acellular matrix is a bone collagen scaffold obtained from natural animal bone containing collagen;
the multiple growth factors are selected from two or more of FGF, VEGF, TGF-β, and BMP.

### Claim 2 (depends on 1)

The bone collagen scaffold material loaded with multiple growth factors according to claim 1, wherein the bone collagen scaffold contains 80 wt %˜98 wt % of collagen, 2 wt %˜10 wt % of miscellaneous proteins, and the rest is hydroxyapatite.

### Claim 3 (depends on 2)

The bone collagen scaffold material loaded with multiple growth factors according to claim 2, wherein the total protein content of the bone collagen scaffold is 84.22 wt %˜98.53 wt %.

### Claim 4 (depends on 3)

The bone collagen scaffold material loaded with multiple growth factors according to claim 3, wherein the bone collagen scaffold contains 96.74 wt % of collagen and 1.79 wt % of miscellaneous proteins, and the pore size on its surface is 60˜70 μm.

### Claim 5 (depends on 1)

The bone collagen scaffold material loaded with multiple growth factors according to claim 1, wherein the bone collagen scaffold material contains four growth factors, namely FGF, VEGF, TGF-β, and BMP, with the loading amounts as follows:
FGF: 20˜27 ng/g,
VEGF: 18˜25 ng/g,
TGF-β: 26˜32 ng/g,
BMP: 24˜30 ng/g.

### Claim 6 (depends on 1)

The bone collagen scaffold material loaded with multiple growth factors according to claim 1, wherein the wet compressive strength of the material is 0.0120˜0.0221 MPa, and the dry compressive strength is 1.25˜2.90 MPa.

### Claim 7 (depends on 1)

A preparation method for the bone collagen scaffold material loaded with multiple growth factors according to claim 1, including the following steps:
1) preparing a bone collagen scaffold: removing surface fat from animal bone, pouring it into a cleaning tank, and placing it in a constant-temperature oscillator for defatting; then, drying and pulverizing the bone, immersing it in a protease solution for 30˜60 min, washing it 8˜10 times with an acidic solution, filtering it out, finally soaking it in purified water for 24˜48 h, draining, and freeze-drying to obtain the bone collagen scaffold;
2) loading growth factors: secondarily pulverizing the bone collagen scaffold prepared in step 1) to a particle size of 1˜10 μm, then immersing it in a growth factor solution for 12˜24 h, centrifuging, discarding a supernatant, pouring it into a mold for freeze-drying, packaging, and sterilizing by irradiation to obtain bone collagen scaffold material.

### Claim 8 (depends on 7)

The preparation method for the bone collagen scaffold material loaded with multiple growth factors according to claim 7, wherein in step 1), when preparing the bone collagen scaffold, defatting solution is a mixture of dichloromethane or chloroform and methanol; the defatting parameters are: temperature: 5˜45° C.: rotation speed: 300˜600 rpm; the defatting solution is a mixture of dichloromethane or chloroform and methanol, with a material-to-liquid ratio of 1:3˜5.

### Claim 9 (depends on 7)

The preparation method for the bone collagen scaffold material loaded with multiple growth factors according to claim 7, wherein in step 1), when preparing the bone collagen scaffold, the acidic solution is hydrochloric acid and/or phosphoric acid with a concentration of 0.5˜1 mol/L; the purified water soaking temperature is 0° C., and the purified water is changed every 12 h during soaking; pH is detected when changing the water, and it is qualified when the pH value is 6˜7.5.

### Claim 10 (depends on 7)

The preparation method for the bone collagen scaffold material loaded with multiple growth factors according to claim 7, wherein in step 2), for loading growth factors, the concentration of the growth factor solution is:
FGF: 30˜50 ng/ml,
VEGF: 25˜40 ng/ml,
TGF-β: 40˜65 ng/ml,
BMP: 40˜65 ng/ml;
the bone collagen scaffold is added to the growth factor solution with a material-to-liquid ratio of 1:5˜10;
the soaking temperature is 0° C.;
the irradiation sterilization dose is 10˜30 kGy.