# US 2026/0048535 A1 · Polymerizing grafted nanoparticles using flow chemistry

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2026/0048535 A1
- Document ID: US20260048535A1
- Status: Published application
- Kind: A1
- Application number: 19/368,756
- Filed: 2025-10-24
- Published: 2026-02-19
- Earliest claimed: 2021-08-17
- Assignees: Honeywell Federal Manufacturing & Technologies, LLC
- Applicants: Honeywell Federal Manufacturing & Technologies, LLC
- Inventors: Sabrina Marie Wells Torres; Laura Christine Cummings; Connor Daniel Pearson
- Web page: https://patentgrep.com/patent/US20260048535A1

## CPC

- B29C 41/02: for making articles of definite length, i.e. discrete articles
- B33Y 70/10: Composites of different types of material, e.g. mixtures of ceramics and polymers or mixtures of metals and biomaterials
- B82Y 30/00: Nanotechnology for materials or surface science, e.g. nanocomposites
- B82Y 40/00: Manufacture or treatment of nanostructures
- C08F 292/00: Macromolecular compounds obtained by polymerising monomers on to inorganic materials
- B29C: SHAPING OR JOINING OF PLASTICS; SHAPING OF MATERIAL IN A PLASTIC STATE, NOT OTHERWISE PROVIDED FOR; AFTER-TREATMENT OF THE SHAPED PRODUCTS, e.g. REPAIRING (making preforms B29B11/00; making laminated products by combining previously unconnected layers which become one product whose layers will remain together B32B37/00 - B32B41/00)
- B33Y: ADDITIVE MANUFACTURING, i.e. MANUFACTURING OF THREE-DIMENSIONAL [3D] OBJECTS BY ADDITIVE DEPOSITION, ADDITIVE AGGLOMERATION OR ADDITIVE LAYERING, e.g. BY 3D PRINTING, STEREOLITHOGRAPHY OR SELECTIVE LASER SINTERING
- B82Y: SPECIFIC USES OR APPLICATIONS OF NANOSTRUCTURES; MEASUREMENT OR ANALYSIS OF NANOSTRUCTURES; MANUFACTURE OR TREATMENT OF NANOSTRUCTURES
- C08F: MACROMOLECULAR COMPOUNDS OBTAINED BY REACTIONS ONLY INVOLVING CARBON-TO-CARBON UNSATURATED BONDS

## Abstract

A process for forming polymer-grafted nanoparticles is provided. The process utilizes flow chemistry techniques to activate nanoparticle surfaces and then form polymer chains on the activated surfaces in a continuous process, thus avoiding the limitations and shortcomings of batch processes for forming polymer-grafted nanoparticles. The polymer-grafted nanoparticles are particularly useful as a filler or additive in fused deposition modeling (“FDM”) filaments, leading to printed parts having improved properties.

## Claims

### Claim 1

A continuous flow process for producing activated nanoparticles, the process comprising:
passing a quantity of starting nanoparticles and a coupling agent through a first channel having a first channel length, wherein said coupling agent bonds with said starting nanoparticles to form the activated nanoparticles within the first channel length; and
passing said activated nanoparticles and a quantity of monomer through a second channel having a second channel length, wherein said monomer polymerizes within the second channel length to form polymer-grafted nanoparticles, said polymer-grafted nanoparticles comprising polymeric chains bonded to said coupling agent.

### Claim 2 (depends on 1)

The process of claim 1, wherein the passing of said activated nanoparticles and quantity of monomer through said second channel length is commenced within about 10 seconds or less after said activated nanoparticles are formed

### Claim 3 (depends on 1)

The process of claim 1, further comprising passing said polymer-grafted nanoparticles through a third channel having a third channel length, wherein said third channel quenches said polymerizing.

### Claim 4 (depends on 3)

The process of claim 3, wherein:
the passing of said activated nanoparticles and quantity of monomer through said second channel length is commenced within about 10 seconds or less after said activated nanoparticles are formed; and
the passing of said polymer-grafted nanoparticles through said third channel length is commenced within about 10 seconds or less after said polymer-grafted nanoparticles are formed.

### Claim 5 (depends on 1)

The process of claim 1, wherein the passing of said starting nanoparticles and coupling agent through said first channel length is completed in about 1 minute to about 3 minutes.

### Claim 6 (depends on 1)

The process of claim 1, wherein the passing of said activated nanoparticles and quantity of monomer through said second channel length is completed in about 5 minutes to about 15 minutes.

### Claim 7 (depends on 3)

The process of claim 3, wherein the passing of said polymer-grafted nanoparticles through said third channel length is completed in about 1 minute to about 4 minutes.

### Claim 8 (depends on 1)

The process of claim 1, wherein said polymer-grafted nanoparticles are formed at a rate of about 0.05 g polymer-grafted nanoparticles/hour or greater.

### Claim 9 (depends on 1)

The process of claim 1, wherein said polymer-grafted nanoparticles have an average grafting density of about 8.488E−05 polymer chains/nm2 of nanoparticle surface area to about 9.62E−03 polymer chains/nm2 of nanoparticle surface area.

### Claim 10 (depends on 1)

The process of claim 1, wherein said starting nanoparticles are chosen from clay nanoparticles, metal oxide nanoparticles, metal nanoparticles, carbonaceous nanoparticles, or mixtures thereof.

### Claim 11 (depends on 1)

The process of claim 1, wherein said coupling agent comprises an alkoxy and a reactive group, said reactive group being chosen from vinyls, epoxies, aminos, acrylics, or mixtures thereof.

### Claim 12 (depends on 1)

The process of claim 1, said monomer comprising at least one group chosen from vinyls, aldehydes, ketones, or mixtures thereof.

### Claim 13 (depends on 1)

The process of claim 1, wherein said first channel comprises a microchannel.

### Claim 14 (depends on 13)

The process of claim 13, wherein said first channel comprises a mixing microchannel section and a reaction microchannel section, wherein:
said mixing microchannel section comprises:
a depth of about 25 μm to about 350 μm;
a width of about 100 μm to about 400 μm; and
a length of about 450 mm to about 600 mm; and
said reaction microchannel section comprises:
a depth of about 25 μm to about 350 μm;
a width of about 200 μm to about 500 μm; and
a length of about 1,000 mm to about 3,000 mm.

### Claim 15 (depends on 13)

The process of claim 13, wherein said first channel has a volume of about 50 μ; to about 1,000 μ;, a length of about 1,450 mm to about 3,600 mm, or both.

### Claim 16 (depends on 13)

The process of claim 13, wherein said second channel comprises a microchannel.

### Claim 17 (depends on 16)

The process of claim 16, wherein said second channel comprises a mixing microchannel section and a reaction microchannel section, wherein:
said mixing microchannel section comprises:
a depth of about 85 μm to about 1,500 μm;
a width of about 85 μm to about 1,500 μm; and
a length of about 450 mm to about 600 mm; and
said reaction microchannel section comprises:
a depth of about 85 μm to about 1,500 μm;
a width of about 200 μm to about 1,500 μm; and
a length of about 1,000 mm to about 3,000 mm.

### Claim 18 (depends on 16)

The process of claim 16, wherein said second channel has a volume of about 500 μl to about 2,000 μl a length of about 1,450 mm to about 3,600 mm, or both.

### Claim 19 (depends on 3)

The process of claim 3, wherein said third channel comprises a microchannel.

### Claim 20 (depends on 19)

The process of claim 19, wherein said third channel has a volume of about 50 μl to about 1,000 μl, a length of about 1,750 mm to about 4,100 mm, or both, said third channel further comprising a mixing microchannel section and a reaction microchannel section, wherein:
said mixing microchannel section comprises:
a depth of about 85 μm to about 1,000 μm;
a width of about 85 μm to about 1,000 μm; and
a length of about 450 mm to about 600 mm; and
said reaction microchannel section comprises:
a depth of about 85 μm to about 1,000 μm;
a width of about 200 μm to about 1.200 μm; and
a length of about 1.300 mm to about 3.500 mm.