# US 2026/0022438 A1 · High strength member, method for manufacturing high strength member, and method for manufacturing steel sheet for high strength member

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2026/0022438 A1
- Document ID: US20260022438A1
- Status: Published application
- Kind: A1
- Application number: 19/339,695
- Filed: 2025-09-25
- Published: 2026-01-22
- Earliest claimed: 2019-05-16
- Assignees: Jfe Steel Corporation
- Applicants: JFE Steel Corporation
- Inventors: Takuya Hirashima; Shinjiro Kaneko
- Web page: https://patentgrep.com/patent/US20260022438A1

## CPC

- C21D 1/22: Martempering
- C21D 9/46: for sheet metals
- C21D 1/26: Methods of annealing
- C21D 6/001: {containing Ni (C21D6/004 takes precedence)}
- C21D 6/002: {containing Cr (C21D6/004 takes precedence)}
- C21D 6/005: {containing Mn}
- C21D 6/008: {containing Si}
- C21D 8/02: during manufacturing of plates or strips (C21D8/12 takes precedence)
- C21D 8/0226: {Hot rolling}
- C21D 8/0236: {Cold rolling}
- C21D 8/0273: {Final recrystallisation annealing}
- C21D 8/0294: involving a localised treatment
- C21D 8/0426: {Hot rolling}
- C21D 8/0436: {Cold rolling}
- C21D 8/0473: {Final recrystallisation annealing}
- C21D 8/0494: {involving a localised treatment}
- C22C 38/00: Ferrous alloys, e.g. steel alloys (cast-iron alloys C22C37/00)
- C22C 38/001: {containing N}
- C22C 38/002: {containing In, Mg, or other elements not provided for in one single group C22C38/001 - C22C38/60}
- C22C 38/005: {containing rare earths, i.e. Sc, Y, Lanthanides}
- C22C 38/02: containing silicon
- C22C 38/04: containing manganese
- C22C 38/06: containing aluminium
- C22C 38/08: containing nickel {(C22C38/105 takes precedence)}
- C22C 38/12: containing tungsten, tantalum, molybdenum, vanadium, or niobium
- C22C 38/14: containing titanium or zirconium
- C22C 38/16: containing copper
- C22C 38/20: with copper
- C22C 38/22: with molybdenum or tungsten
- C22C 38/24: with vanadium
- C22C 38/26: with niobium or tantalum
- C22C 38/38: with more than 1.5% by weight of manganese
- C22C 38/60: containing lead, selenium, tellurium, or antimony, or more than 0.04% by weight of sulfur
- B21D 5/008: {combined with heating or cooling of the bends}
- C21D 1/30: Stress-relieving
- C21D 7/10: of the whole cross-section, e.g. of concrete reinforcing bars
- C21D 8/0221: characterised by the working steps
- C21D 8/0247: characterised by the heat treatment
- C21D 2211/002: Bainite
- C21D 2211/008: Martensite
- C21D 2221/01: End parts (e.g. leading, trailing end)
- C21D 2221/02: Edge parts
- C21D 2261/00: Machining or cutting being involved
- Y02P 10/20: Recycling
- C21D: MODIFYING THE PHYSICAL STRUCTURE OF FERROUS METALS; GENERAL DEVICES FOR HEAT TREATMENT OF FERROUS OR NON-FERROUS METALS OR ALLOYS; MAKING METAL MALLEABLE, e.g. BY DECARBURISATION OR TEMPERING (surface treatment of metallic material involving at least one process provided for in class C23 and at least one process covered by this subclass C23F17/00; unidirectional solidification of eutectic materials or unidirectional demixing of eutectoid materials C30B)
- C22C: ALLOYS (treatment of alloys C21D, C22F)
- B21D: WORKING OR PROCESSING OF SHEET METAL OR METAL TUBES, RODS OR PROFILES WITHOUT ESSENTIALLY REMOVING MATERIAL; PUNCHING METAL (working or processing of wire B21F)
- Y02P: CLIMATE CHANGE MITIGATION TECHNOLOGIES IN THE PRODUCTION OR PROCESSING OF GOODS

## Abstract

A high strength member according to the present invention is the high strength member having a bending ridge line portion formed from a steel sheet, the member having a tensile strength of 1470 MPa or higher, a residual stress of 300 MPa or lower in an end surface of the bending ridge line portion, and a Vickers hardness (HV) of 200 or higher and 450 or lower in the end surface of the bending ridge line portion.

## Claims

### Claim 1

A method for manufacturing a high strength member, the method comprising
a bending work process of cutting a steel sheet having a tensile strength of 1470 MPa or higher and performing bending work on the cut steel sheet and
an end surface treatment process of heating an end surface, which has been formed by cutting, at a temperature of 400° C. or higher and 900° C. or lower for more than 0 seconds and 10 seconds or less after the bending work process.

### Claim 2 (depends on 1)

The method according to claim 1, wherein the steel sheet has a chemical composition containing, by mass %,
C: 0.17% or more and 0.35% or less,
Si: 0.001% or more and 1.2% or less,
Mn: 0.9% or more and 3.2% or less,
P: 0.020% or less,
S: 0.0010% or less,
Al: 0.010% or more and 0.20% or less,
N: 0.010% or less, and a balance of Fe and incidental impurities, and
a microstructure, in which a total area fraction of one or both of bainite containing carbides having an average grain size of 50 nm or less and martensite containing carbides having an average grain size of 50 nm or less is 90% or more.

### Claim 3 (depends on 1)

The method according to claim 1, wherein the steel sheet has a chemical composition containing, by mass %,
C: 0.17% or more and 0.35% or less,
Si: 0.001% or more and 1.2% or less,
Mn: 0.9% or more and 3.2% or less,
P: 0.020% or less,
S: 0.0010% or less,
Al: 0.010% or more and 0.20% or less,
N: 0.010% or less,
Sb: 0.001% or more and 0.10% or less, and a balance of Fe and incidental impurities, and
a microstructure, in which a total area fraction of one or both of bainite containing carbides having an average grain size of 50 nm or less and martensite containing carbides having an average grain size of 50 nm or less is 90% or more.

### Claim 4 (depends on 2)

The method according to claim 2, wherein the steel sheet has the chemical composition further containing at least one selected from the groups of, by mass %,
group A:
B: 0.0002% or more and less than 0.0035%,
group B:
at least one selected from
Nb: 0.002% or more and 0.08% or less, and
Ti: 0.002% or more and 0.12% or less,
group C:
at least one selected from
Cu: 0.005% or more and 18 or less, and
Ni: 0.005% or more and 1% or less,
group D:
at least one selected from
Cr: 0.01% or more and 1.0% or less,
Mo: 0.01% or more and less than 0.3%,
V: 0.003% or more and 0.5% or less,
Zr: 0.005% or more and 0.20% or less, and
W: 0.005% or more and 0.20% or less,
group E:
at least one selected from
Ca: 0.0002% or more and 0.0030% or less,
Ce: 0.0002% or more and 0.0030% or less,
La: 0.0002% or more and 0.0030% or less, and
Mg: 0.0002% or more and 0.0030% or less, and
group F:
Sn: 0.002% or more and 0.1% or less.

### Claim 5 (depends on 3)

The method according to claim 3, wherein the steel sheet has the chemical composition further containing at least one selected from the groups of, by mass %,
group A:
B: 0.0002% or more and less than 0.0035%,
group B:
at least one selected from
Nb: 0.002% or more and 0.08% or less, and
Ti: 0.002% or more and 0.12% or less,
group C:
at least one selected from
Cu: 0.005% or more and 18 or less, and
Ni: 0.005% or more and 18 or less,
group D:
at least one selected from
Cr: 0.01% or more and 1.08 or less,
Mo: 0.01% or more and less than 0.3%,
V: 0.003% or more and 0.5% or less,
Zr: 0.005% or more and 0.20% or less, and
W: 0.005% or more and 0.20% or less,
group E:
at least one selected from
Ca: 0.0002% or more and 0.0030% or less,
Ce: 0.0002% or more and 0.0030% or less,
La: 0.0002% or more and 0.0030% or less, and
Mg: 0.0002% or more and 0.0030% or less, and
group F:
Sn: 0.002% or more and 0.1% or less.

### Claim 6

A method for manufacturing a high strength member, the method comprising
an end surface treatment process of cutting a steel sheet having a tensile strength of 1470 MPa or higher and heating an end surface, which has been formed by cutting, at a temperature of 400° C. or higher and 900° C. or lower for more than 0 seconds and 10 seconds or less and
a bending work process of performing bending work on the steel sheet, which has been subjected to the end surface treatment process.

### Claim 7 (depends on 6)

The method according to claim 6, wherein the steel sheet has a chemical composition containing, by mass %,
C: 0.17% or more and 0.35% or less,
Si: 0.001% or more and 1.2% or less,
Mn: 0.9% or more and 3.2% or less,
P: 0.020% or less,
S: 0.0010% or less,
Al: 0.010% or more and 0.20% or less,
N: 0.010% or less, and a balance of Fe and incidental impurities, and
a microstructure, in which a total area fraction of one or both of bainite containing carbides having an average grain size of 50 nm or less and martensite containing carbides having an average grain size of 50 nm or less is 90% or more.

### Claim 8 (depends on 6)

The method according to claim 6, wherein the steel sheet has a chemical composition containing, by mass %,
C: 0.17% or more and 0.35% or less,
Si: 0.001% or more and 1.2% or less,
Mn: 0.9% or more and 3.2% or less,
P: 0.020% or less,
S: 0.0010% or less,
Al: 0.010% or more and 0.20% or less,
N: 0.010% or less,
Sb: 0.001% or more and 0.10% or less, and a balance of Fe and incidental impurities, and
a microstructure, in which a total area fraction of one or both of bainite containing carbides having an average grain size of 50 nm or less and martensite containing carbides having an average grain size of 50 nm or less is 90% or more.

### Claim 9 (depends on 7)

The method according to claim 7, wherein the steel sheet has the chemical composition further containing at least one selected from the groups of, by mass %,
group A:
B: 0.0002% or more and less than 0.0035%,
group B:
at least one selected from
Nb: 0.002% or more and 0.08% or less, and
Ti: 0.002% or more and 0.12% or less,
group C:
at least one selected from
Cu: 0.005% or more and 18 or less, and
Ni: 0.005% or more and 1% or less,
group D:
at least one selected from
Cr: 0.01% or more and 1.0% or less,
Mo: 0.01% or more and less than 0.3%,
V: 0.003% or more and 0.5% or less,
Zr: 0.005% or more and 0.20% or less, and
W: 0.005% or more and 0.20% or less,
group E:
at least one selected from
Ca: 0.0002% or more and 0.0030% or less,
Ce: 0.0002% or more and 0.0030% or less,
La: 0.0002% or more and 0.0030% or less, and
Mg: 0.0002% or more and 0.0030% or less, and
group F:
Sn: 0.0028 or more and 0.1% or less.

### Claim 10 (depends on 8)

The method according to claim 8, wherein the steel sheet has the chemical composition further containing at least one selected from the groups of, by mass %,
group A:
B: 0.0002% or more and less than 0.0035%,
group B:
at least one selected from
Nb: 0.002% or more and 0.08% or less, and
Ti: 0.002% or more and 0.12% or less,
group C:
at least one selected from
Cu: 0.005% or more and 18 or less, and
Ni: 0.005% or more and 18 or less,
group D:
at least one selected from
Cr: 0.01% or more and 1.0% or less,
Mo: 0.01% or more and less than 0.3%,
V: 0.003% or more and 0.5% or less,
Zr: 0.005% or more and 0.20% or less, and
W: 0.005% or more and 0.20% or less,
group E:
at least one selected from
Ca: 0.0002% or more and 0.0030% or less,
Ce: 0.0002% or more and 0.0030% or less,
La: 0.0002% or more and 0.0030% or less, and
Mg: 0.0002% or more and 0.0030% or less, and
group F:
Sn: 0.002% or more and 0.1% or less.

### Claim 11 (depends on 1)

A method for manufacturing a steel sheet for the high strength member manufactured by using the method for manufacturing a high strength member according to claim 1, the method for manufacturing a steel sheet comprising
a hot rolling process of performing hot rolling on a steel material,
a cold rolling process of performing cold rolling on a hot rolled steel sheet, which has been obtained by performing the hot rolling process, and
an annealing process of heating a cold rolled steel sheet, which has been obtained by performing the cold rolling process, to an annealing temperature equal to or higher than an Ac3 temperature, cooling the heated steel sheet to a cooling stop temperature of 350° C. or lower at an average cooling rate of 3° C./sec or higher in a temperature range from the annealing temperature to a temperature of 550° C., and holding the cooled steel sheet in a temperature range of 100° C. or higher and 260° C. or lower for 20 seconds or more and 1500 seconds or less.

### Claim 12 (depends on 2)

A method for manufacturing a steel sheet for the high strength member manufactured by using the method for manufacturing a high strength member according to claim 2, the method for manufacturing a steel sheet comprising
a hot rolling process of performing hot rolling on a steel material,
a cold rolling process of performing cold rolling on a hot rolled steel sheet, which has been obtained by performing the hot rolling process, and
an annealing process of heating a cold rolled steel sheet, which has been obtained by performing the cold rolling process, to an annealing temperature equal to or higher than an Ac3 temperature, cooling the heated steel sheet to a cooling stop temperature of 350° C. or lower at an average cooling rate of 3° C./sec or higher in a temperature range from the annealing temperature to a temperature of 550° C., and holding the cooled steel sheet in a temperature range of 100° C. or higher and 260° C. or lower for 20 seconds or more and 1500 seconds or less.

### Claim 13 (depends on 3)

A method for manufacturing a steel sheet for the high strength member manufactured by using the method for manufacturing a high strength member according to claim 3, the method for manufacturing a steel sheet comprising
a hot rolling process of performing hot rolling on a steel material,
a cold rolling process of performing cold rolling on a hot rolled steel sheet, which has been obtained by performing the hot rolling process, and
an annealing process of heating a cold rolled steel sheet, which has been obtained by performing the cold rolling process, to an annealing temperature equal to or higher than an Ac3 temperature, cooling the heated steel sheet to a cooling stop temperature of 350° C. or lower at an average cooling rate of 3° C./sec or higher in a temperature range from the annealing temperature to a temperature of 550° C., and holding the cooled steel sheet in a temperature range of 100° C. or higher and 260° C. or lower for 20 seconds or more and 1500 seconds or less.

### Claim 14 (depends on 4)

A method for manufacturing a steel sheet for the high strength member manufactured by using the method for manufacturing a high strength member according to claim 4, the method for manufacturing a steel sheet comprising
a hot rolling process of performing hot rolling on a steel material,
a cold rolling process of performing cold rolling on a hot rolled steel sheet, which has been obtained by performing the hot rolling process, and
an annealing process of heating a cold rolled steel sheet, which has been obtained by performing the cold rolling process, to an annealing temperature equal to or higher than an Ac3 temperature, cooling the heated steel sheet to a cooling stop temperature of 350° C. or lower at an average cooling rate of 3° C./sec or higher in a temperature range from the annealing temperature to a temperature of 550° C., and holding the cooled steel sheet in a temperature range of 100° C. or higher and 260° C. or lower for 20 seconds or more and 1500 seconds or less.

### Claim 15 (depends on 5)

A method for manufacturing a steel sheet for the high strength member manufactured by using the method for manufacturing a high strength member according to claim 5, the method for manufacturing a steel sheet comprising
a hot rolling process of performing hot rolling on a steel material,
a cold rolling process of performing cold rolling on a hot rolled steel sheet, which has been obtained by performing the hot rolling process, and
an annealing process of heating a cold rolled steel sheet, which has been obtained by performing the cold rolling process, to an annealing temperature equal to or higher than an Ac3 temperature, cooling the heated steel sheet to a cooling stop temperature of 350° C. or lower at an average cooling rate of 3° C./sec or higher in a temperature range from the annealing temperature to a temperature of 550° C., and holding the cooled steel sheet in a temperature range of 100° C. or higher and 260° C. or lower for 20 seconds or more and 1500 seconds or less.

### Claim 16 (depends on 6)

A method for manufacturing a steel sheet for the high strength member manufactured by using the method for manufacturing a high strength member according to claim 6, the method for manufacturing a steel sheet comprising
a hot rolling process of performing hot rolling on a steel material,
a cold rolling process of performing cold rolling on a hot rolled steel sheet, which has been obtained by performing the hot rolling process, and
an annealing process of heating a cold rolled steel sheet, which has been obtained by performing the cold rolling process, to an annealing temperature equal to or higher than an Ac3 temperature, cooling the heated steel sheet to a cooling stop temperature of 350° C. or lower at an average cooling rate of 3° C./sec or higher in a temperature range from the annealing temperature to a temperature of 550° C., and holding the cooled steel sheet in a temperature range of 100° C. or higher and 260° C. or lower for 20 seconds or more and 1500 seconds or less.

### Claim 17 (depends on 7)

A method for manufacturing a steel sheet for the high strength member manufactured by using the method for manufacturing a high strength member according to claim 7, the method for manufacturing a steel sheet comprising
a hot rolling process of performing hot rolling on a steel material,
a cold rolling process of performing cold rolling on a hot rolled steel sheet, which has been obtained by performing the hot rolling process, and
an annealing process of heating a cold rolled steel sheet, which has been obtained by performing the cold rolling process, to an annealing temperature equal to or higher than an Ac3 temperature, cooling the heated steel sheet to a cooling stop temperature of 350° C. or lower at an average cooling rate of 3° C./sec or higher in a temperature range from the annealing temperature to a temperature of 550° C., and holding the cooled steel sheet in a temperature range of 100° C. or higher and 260° C. or lower for 20 seconds or more and 1500 seconds or less.

### Claim 18 (depends on 8)

A method for manufacturing a steel sheet for the high strength member manufactured by using the method for manufacturing a high strength member according to claim 8, the method for manufacturing a steel sheet comprising
a hot rolling process of performing hot rolling on a steel material,
a cold rolling process of performing cold rolling on a hot rolled steel sheet, which has been obtained by performing the hot rolling process, and
an annealing process of heating a cold rolled steel sheet, which has been obtained by performing the cold rolling process, to an annealing temperature equal to or higher than an Ac3 temperature, cooling the heated steel sheet to a cooling stop temperature of 350° C. or lower at an average cooling rate of 3° C./sec or higher in a temperature range from the annealing temperature to a temperature of 550° C., and holding the cooled steel sheet in a temperature range of 100° C. or higher and 260° C. or lower for 20 seconds or more and 1500 seconds or less.

### Claim 19 (depends on 9)

A method for manufacturing a steel sheet for the high strength member manufactured by using the method for manufacturing a high strength member according to claim 9, the method for manufacturing a steel sheet comprising
a hot rolling process of performing hot rolling on a steel material,
a cold rolling process of performing cold rolling on a hot rolled steel sheet, which has been obtained by performing the hot rolling process, and
an annealing process of heating a cold rolled steel sheet, which has been obtained by performing the cold rolling process, to an annealing temperature equal to or higher than an Ac3 temperature, cooling the heated steel sheet to a cooling stop temperature of 350° C. or lower at an average cooling rate of 3° C./sec or higher in a temperature range from the annealing temperature to a temperature of 550° C., and holding the cooled steel sheet in a temperature range of 100° C. or higher and 260° C. or lower for 20 seconds or more and 1500 seconds or less.

### Claim 20 (depends on 10)

A method for manufacturing a steel sheet for the high strength member manufactured by using the method for manufacturing a high strength member according to claim 10, the method for manufacturing a steel sheet comprising
a hot rolling process of performing hot rolling on a steel material,
a cold rolling process of performing cold rolling on a hot rolled steel sheet, which has been obtained by performing the hot rolling process, and
an annealing process of heating a cold rolled steel sheet, which has been obtained by performing the cold rolling process, to an annealing temperature equal to or higher than an Ac3 temperature, cooling the heated steel sheet to a cooling stop temperature of 350° C. or lower at an average cooling rate of 3° C./sec or higher in a temperature range from the annealing temperature to a temperature of 550° C., and holding the cooled steel sheet in a temperature range of 100° C. or higher and 260° C. or lower for 20 seconds or more and 1500 seconds or less.