# US 2026/0015694 A1 · Porous metal structure and preparation method for the same

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2026/0015694 A1
- Document ID: US20260015694A1
- Status: Published application
- Kind: A1
- Application number: 19/332,972
- Filed: 2025-09-18
- Published: 2026-01-15
- Earliest claimed: 2023-12-29
- Assignees: Contemporary Amperex Technology Co., Limited
- Applicants: Contemporary Amperex Technology Co., Limited
- Inventors: Zun LI; Manman WANG; Xiaoming GE; Chuying OUYANG
- Web page: https://patentgrep.com/patent/US20260015694A1

## CPC

- C22C 1/088: {Foaming process with solid metal other than by powder metallurgy}
- H01M 4/662: {Alloys (collectors of lead alloys H01M4/685)}
- C22C 9/00: Alloys based on copper
- C22C 9/05: with manganese as the next major constituent
- C22F 1/02: in inert or controlled atmosphere or vacuum (adjusting the composition of the atmosphere C21D1/76)
- C22F 1/057: of alloys with copper as the next major constituent
- C22F 1/08: of copper or alloys based thereon
- C23F 1/00: Etching metallic material by chemical means (manufacture of printing surfaces B41C; manufacture of printed circuits H05K)
- H01M 4/742: {perforated material}
- C25F 3/02: Etching
- C22C: ALLOYS (treatment of alloys C21D, C22F)
- H01M: PROCESSES OR MEANS, e.g. BATTERIES, FOR THE DIRECT CONVERSION OF CHEMICAL ENERGY INTO ELECTRICAL ENERGY
- C22F: CHANGING THE PHYSICAL STRUCTURE OF NON-FERROUS METALS AND NON-FERROUS ALLOYS (surface treatment of metallic material involving at least one process provided for in class C23 and at least one process covered by this subclass, C23F17/00)
- C23F: NON-MECHANICAL REMOVAL OF METALLIC MATERIAL FROM SURFACE (working metal by laser beams B23K26/00; desurfacing by applying flames B23K7/00; working of metal by electro-erosion B23H; producing decorative effects by removing surface material, e.g. by engraving, by etching, B44C1/22; electrolytic etching or polishing C25F); INHIBITING CORROSION OF METALLIC MATERIAL OR INCRUSTATION IN GENERAL; MULTI-STEP PROCESSES FOR SURFACE TREATMENT OF METALLIC MATERIAL INVOLVING AT LEAST ONE PROCESS PROVIDED FOR IN CLASS C23 AND AT LEAST ONE PROCESS COVERED BY SUBCLASS C21D OR C22F OR CLASS C25
- C25F: PROCESSES FOR THE ELECTROLYTIC REMOVAL OF MATERIALS FROM OBJECTS; APPARATUS THEREFOR

## Abstract

A porous metal structure and a preparation method for the same. The preparation method for the porous metal structure includes the following steps: performing first de-alloying treatment on an alloy foil to form pores, then performing reduction annealing treatment in a reducing gas atmosphere, and finally performing second de-alloying treatment to obtain the porous metal structure.

## Claims

### Claim 1

A preparation method for a porous metal structure, comprising:
performing first de-alloying treatment on an alloy foil to form pores, then performing reduction annealing treatment in a reducing gas atmosphere, and finally performing second de-alloying treatment to obtain the porous metal structure.

### Claim 2 (depends on 1)

The preparation method according to claim 1, wherein:
a process for the first de-alloying treatment comprises a free-corrosion de-alloying process or an electrochemical-corrosion de-alloying process, and a process for the second de-alloying treatment comprises the free-corrosion de-alloying process; and
the process for the first de-alloying treatment comprises the free-corrosion de-alloying process, and the process for the second de-alloying treatment comprises the free-corrosion de-alloying process.

### Claim 3 (depends on 1)

The preparation method according to claim 1, wherein the process for the first de-alloying treatment comprises the free-corrosion de-alloying process, the process for the second de-alloying treatment comprises the free-corrosion de-alloying process, corrosion solutions used in the first de-alloying treatment and the second de-alloying treatment are acidic solutions, and the acidic solutions comprise an acidic aqueous solution, and further comprise one or a mixture of more of hydrochloric acid, sulfuric acid, phosphoric acid, and acetic acid.

### Claim 4 (depends on 3)

The preparation method according to claim 3, wherein:
a concentration C1 of the acidic solution used in the first de-alloying treatment is greater than a concentration C2 of the acidic solution used in the second de-alloying treatment; and/or
a treatment temperature T1 of the first de-alloying treatment is greater than a treatment temperature T2 of the second de-alloying treatment, T1 ranges from 40° C. to 80° C., and T2 ranges from 20° C. to 30° C.; and/or
a treatment time t1 of the first de-alloying treatment is greater than a treatment time t2 of the second de-alloying treatment, t1 is greater than or equal to 24 h, and t2 is less than or equal to 12 h.

### Claim 5 (depends on 1)

The preparation method according to claim 1, wherein the reduction annealing treatment satisfies at least one of the following conditions (1) to (8):
(1) a reducing gas used in the reduction annealing treatment comprises ammonia gas or a mixture of hydrogen gas and inert gas;
(2) the reducing gas used in the reduction annealing treatment comprises a mixture of hydrogen gas and inert gas, and the inert gas comprises one or more of nitrogen gas, argon gas, and helium gas;
(3) a flow rate of the reducing gas used in the reduction annealing treatment ranges from 100 SCCM to 2000 SCCM;
(4) the reduction annealing treatment is performed in a tube furnace, and a heating rate of the tube furnace ranges from 2° C./min to 10° C./min;
(5) the reduction annealing treatment is performed in a tube furnace, and a heating rate of the tube furnace ranges from 5° C./min to 10° C./min;
(6) an average cooling rate of a cooling treatment process after the reduction annealing treatment is less than or equal to 2° C./min;
(7) the cooling treatment process is a furnace cooling process; and
(8) cooling treatment after the reduction annealing treatment comprises cooling to 50° C. or below.

### Claim 6 (depends on 1)

The preparation method according to claim 1, wherein the alloy foil is a copper alloy foil, the copper alloy foil comprises a Cu element and a non-Cu metal element, and a standard electrode potential of the non-Cu metal element is lower than a standard electrode potential of the Cu element, wherein:
the non-Cu metal element comprises one or more of Mn, Zn, Ni, Al, and Fe; and/or
an atomic content of the non-Cu metal element in the copper alloy foil is 60 at. % or more, or ranges from 65 at. % to 80 at. %.

### Claim 7 (depends on 1)

The preparation method according to claim 1, wherein:
a holding temperature for the reduction annealing treatment ranges from 700° C. to 900° C.; and/or
a holding time at the temperature of the reduction annealing treatment ranges from 20 min to 60 min.

### Claim 8 (depends on 1)

The preparation method according to claim 1, further comprising, before the first de-alloying treatment is performed on the alloy foil:
providing a cold-rolled alloy foil;
performing recrystallization annealing treatment on the alloy foil, and then performing first cooling treatment to obtain an alloy foil with a first component phase; and
performing phase separation heat treatment on the alloy foil with the first component phase, and then performing second cooling treatment to precipitate a second component phase and obtain an alloy foil with the first component phase and the second component phase, wherein a temperature of the phase separation heat treatment is less than a temperature of the recrystallization annealing treatment, and an average cooling rate of the second cooling treatment is less than an average cooling rate of the first cooling treatment.

### Claim 9 (depends on 8)

The preparation method according to claim 8, wherein:
the average cooling rate of the first cooling treatment is greater than or equal to 100° C./min, or greater than or equal to 200° C./min; and/or
the average cooling rate of the second cooling treatment is less than or equal to 2° C./min.

### Claim 10 (depends on 8)

The preparation method according to claim 8, wherein:
a process for the first cooling treatment is a water cooling process; and/or
a process for the second cooling treatment is a furnace cooling process.

### Claim 11 (depends on 8)

The preparation method according to claim 8, wherein:
the first cooling treatment comprises cooling to 50° C. or below; and/or
the second cooling treatment comprises cooling to 50° C. or below.

### Claim 12 (depends on 8)

The preparation method according to claim 8, wherein:
the recrystallization annealing treatment is performed in a muffle furnace; and/or
the phase separation heat treatment is performed in a tube furnace, and a heating rate of the tube furnace ranges from 2° C./min to 10° C./min, or ranges from 5° C./min to 10° C./min.

### Claim 13 (depends on 8)

The preparation method according to claim 8, wherein:
a temperature of the recrystallization annealing treatment ranges from 720° C. to 850° C.; and/or
a holding time at the temperature of the recrystallization annealing treatment ranges from 10 min to 60 min; and/or
a temperature of the phase separation heat treatment ranges from 620° C. to 700° C.; and/or
a holding time at the temperature of the phase separation heat treatment ranges from 60 min to 360 min.

### Claim 14 (depends on 8)

The preparation method according to claim 8, wherein:
the first component phase comprises a gamma phase; and/or
the second component phase comprises an alpha phase.

### Claim 15 (depends on 1)

A porous metal structure prepared by the preparation method according to claim 1.

### Claim 16 (depends on 15)

The porous metal structure according to claim 15, wherein the porous metal structure is a porous copper structure, the porous copper structure comprises a non-Cu metal element, and an atomic content of the non-Cu metal element is 0.3 wt % or less, or 0.2 wt % or less.