# US 2025/0385018 A1 · Composition comprising dual chem-heat treated brine sludge waste for flexible and moldable material and a process for the preparation thereof

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2025/0385018 A1
- Document ID: US20250385018A1
- Status: Published application
- Kind: A1
- Application number: 19/236,383
- Filed: 2025-06-12
- Published: 2025-12-18
- Earliest claimed: 2024-06-13
- Assignees: Council of Scientific and Industrial Research
- Applicants: Council of Scientific & Industrial Research
- Inventors: Sarika VERMA; Medha MILI; Mohammed Akram KHAN; Avanish Kumar SRIVASTAVA
- Web page: https://patentgrep.com/patent/US20250385018A1

## CPC

- G21F 1/103: {Dispersions in organic carriers}
- C02F 11/008: {Sludge treatment by fixation or solidification}
- C02F 11/13: by heating
- G21F: PROTECTION AGAINST X-RADIATION, GAMMA RADIATION, CORPUSCULAR RADIATION OR PARTICLE BOMBARDMENT; TREATING RADIOACTIVELY CONTAMINATED MATERIAL; DECONTAMINATION ARRANGEMENTS THEREFOR (radiation protection by pharmaceutical means A61K8/00, A61Q17/04; in cosmonautic vehicles B64G1/54; combined with a reactor G21C11/00; combined with X-ray tubes H01J35/16; combined with X-ray apparatus H05G1/02)
- C02F: TREATMENT OF WATER, WASTE WATER, SEWAGE, OR SLUDGE (separation in general B01D; special arrangements on waterborne vessels of installations for treating water, waste water or sewage, e.g. for producing fresh water, B63J; adding materials to water to prevent corrosion C23F; treating radioactively-contaminated liquids G21F9/04; regeneration of reactants for recirculation into processes, see the relevant places for the processes)

## Abstract

The present invention provides a composition for material comprising brine sludge waste and a process for the preparation thereof process for preparation of flexible, functional, and moldable material using advanced Chem-heat treated brine sludge-based composition via solvent-free route for developing samples of various dimensions. The present invention involves developing desired, suitable, and appropriate phases possessing uniform and homogenous matrix in the developed material. Thus, designing molecular moieties in the developed process leads to forming tightly bound three-dimensional structures, strengthening the developed advanced chemically designed material which is cost-effective, non-toxic, highly versatile (can be bent or shaped to fit around curves and corners), durable, easy to install, safe with superior performance and economically feasible advanced flexible, functional and moldable material with a homogeneous uniform matrix using advanced dual chem-heat treated brine sludge based composition for a broad application spectrum.

## Claims

### Claim 1

A composition for dual chem-heat treated brine sludge waste for flexible and moldable radiation shielding material, wherein the composition comprising:
(a) advanced brine sludge based tailored material;
(b) polymeric cis-1,4-polyisoprene (2-methyl-1,3-butadiene) or polymerized Acrylonitrile (CH2═CHCN) and Butadiene (CH2CH—CH—CH2);
(c) oil;
(d) carbon;
(e) sulphur;
(f) tetramethyl thiuram disulphide;
(g) 2-mercaptobenzothiazole; and
(h) Stearic Acid;
wherein the ratio of [a]:[b]:[c]:[d]:[e]:[f]:[g]:[h] ranges from 71.16 to 80.95:12.95 to 25.62:1.66 to 4.44:1.11 to 2.96:0.08 to 0.22:0.03 to 0.15:0.11 to 0.29:0.11 to 0.29.

### Claim 2 (depends on 1)

The composition as claimed in claim 1, wherein the ratio of ratio of [a]:[b]:[c]:[d]:[e]:[f]:[g]:[h] is 71.16:25.62:1.71:1.14:0.09:0.06:0.11:0.11.

### Claim 3 (depends on 1)

The composition as claimed in claim 1, wherein the advanced brine sludge-based tailored material comprises:
(i) brine Sludge;
(ii) sodium hexametaphosphate; and
(iii) bismuth oxide powder;
wherein the ratio of [i]:[ii]:[iii] ranges from 61.54 to 75.00:8.85 to 25.00:0.1 to 20.35.

### Claim 4 (depends on 1)

The composition as claimed in claim 1, wherein the ratio of Brine Sludge:Sodium hexametaphosphate:Bismuth Oxide powder in the advanced brine sludge based tailored material is 61.54:8.85:0.1.

### Claim 5

A process for the preparation of dual chem-heat treated brine sludge waste material for flexible and moldable material comprising the following steps:
a) grinding of brine sludge, Sodium Hexametaphosphate (SHMP) for a period of 2-3 hours to obtain a material followed by compacting and heating the obtained material at 900 to 1000° C. in a furnace for a duration of 1-1.5 hours to obtain heat-treated material;
b) grinding the heat-treated material obtained in step (a) along with 120-230 g bismuth oxide powder for a period of 2-2.5 hours to obtain advanced brine sludge based tailored material;
c) mixing the advanced brine sludge based tailored material obtained in step (b) with polymeric cis-1,4-polyisoprene (2-methyl-1,3-butadiene) or polymerized acrylonitrile (CH2═CHCN) and butadiene (CH2CH—CH—CH2) and rolling for a duration of 10 to 15 minutes, followed by adding oil, carbon, sulfur, tetramethyl thiuram disulphide,2-mercaptobenzothiazole, stearic acid and mixing thoroughly and rolling for 15 to 20 minutes to obtain a mixture;
d) cooling and molding the mixture obtained in step [c] followed by pressing for a duration of 6 to 9 minutes at a temperature in the range of 120 to 130° C. and demolding to obtain the desired flexible, functional and moldable radiation shielding material.