# US 2025/0320575 A1 · Non-oriented electrical steel and a method of manufacturing non-oriented electrical steel thereof

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2025/0320575 A1
- Document ID: US20250320575A1
- Status: Published application
- Kind: A1
- Application number: 19/246,103
- Filed: 2025-06-23
- Published: 2025-10-16
- Earliest claimed: 2023-11-15
- Assignees: ArcelorMittal
- Applicants: ArcelorMittal
- Inventors: Sigrid JACOBS; Xavier CHASSANG; Elke LEUNIS
- Web page: https://patentgrep.com/patent/US20250320575A1

## CPC

- C21D 9/46: for sheet metals
- C22C 38/02: containing silicon
- C21D 1/26: Methods of annealing
- C21D 6/008: {containing Si}
- C21D 8/1205: involving particular fabrication steps or treatments of ingots or slabs
- C21D 8/1222: {Hot rolling}
- C21D 8/1233: {Cold rolling}
- C21D 8/1244: characterised by the heat treatment
- C21D 8/1261: {following hot rolling}
- C21D 8/1272: {Final recrystallisation annealing}
- C21D 8/1283: {Application of a separating or insulating coating}
- C22C 38/001: {containing N}
- C22C 38/002: {containing In, Mg, or other elements not provided for in one single group C22C38/001 - C22C38/60}
- C22C 38/004: {Very low carbon steels, i.e. having a carbon content of less than 0,01%}
- C22C 38/04: containing manganese
- C22C 38/06: containing aluminium
- C22C 38/20: with copper
- C22C 38/34: with more than 1.5% by weight of silicon
- H01F 1/14791: {Fe-Si-Al based alloys, e.g. Sendust}
- C21D 2211/005: Ferrite
- C22C 2202/02: Magnetic
- C21D: MODIFYING THE PHYSICAL STRUCTURE OF FERROUS METALS; GENERAL DEVICES FOR HEAT TREATMENT OF FERROUS OR NON-FERROUS METALS OR ALLOYS; MAKING METAL MALLEABLE, e.g. BY DECARBURISATION OR TEMPERING (surface treatment of metallic material involving at least one process provided for in class C23 and at least one process covered by this subclass C23F17/00; unidirectional solidification of eutectic materials or unidirectional demixing of eutectoid materials C30B)
- C22C: ALLOYS (treatment of alloys C21D, C22F)
- H01F: MAGNETS; INDUCTANCES; TRANSFORMERS; SELECTION OF MATERIALS FOR THEIR MAGNETIC PROPERTIES

## Abstract

A non-oriented electrical steel sheet having a composition of the following elements, expressed in percentage by weight 0.0001%≤Carbon≤0.007%, 0.15%≤Manganese≤0.25%, 2.9%≤Silicon≤3.4%, 0.8%≤Aluminum≤1.1%, Phosphorus≤0.15%, Sulfur≤0.006%, Nitrogen≤0.09%, with 3.85%≤Si+Al+Mn≤5.5%, and the following optional elements 0%≤Niobium≤0.1%, 0%≤Titanium≤0.1%, 0%≤Vanadium≤0.1%, 0%≤Chromium≤1%, 0%≤Molybdenum≤0.5%, 0%≤Tungsten≤0.1%, 0%≤Cobalt≤1%, 0%≤Arsenic≤0.05%, 0.001%≤Calcium≤0.01%, 0%≤Copper≤1%, 0%≤Nickel≤1%, 0%≤Boron≤0.05%, 0%≤Lead≤0.2%, 0%≤Tin≤0.2%, 0%≤Antimony≤0.2%, the remainder composition being composed of iron and unavoidable impurities caused by processing. The microstructure is made of ferrite and including in area fraction, 80% to 100% recrystallized microstructure, 0% to 20% non-recrystallized microstructure wherein the average grain size of recrystallized microstructure is from 20 microns to 110 microns and having a percentage of eddy current losses in total iron losses less than 25% and simultaneously having a magnetic polarization at 5000 A/m from 1.625 T to 1.690 T.

## Claims

### Claim 1

A non-oriented electrical steel sheet having a composition comprising of the following elements, expressed in percentage by weight:
0.0001
%
≤
Carbon
≤
0.007
%
0.15
%
≤
Manganese
≤
0.25
3.1
%
≤
Silicon
≤
3.3
%
0.8
%
≤
Aluminum
≤
1.1
%
Phosphorus
≤
0.15
%
Sulfur
≤
0.006
%
Nitrogen
≤
0.09
%
with
3.85
%
≤
Si
+
Al
+
Mn
≤
5.5
%
and optionally or more of the following elements:
0
⁢
%
≤
Niobium
≤
0.1
%
0
⁢
%
≤
Titanium
≤
0.1
%
0
⁢
%
≤
Vanadium
≤
0.1
%
0
⁢
%
≤
Chromium
≤
1
⁢
%
0
⁢
%
≤
Molybdenum
≤
0.5
%
0
⁢
%
≤
Tungsten
≤
0.
%
0
⁢
%
≤
Cobalt
≤
1
⁢
%
0
⁢
%
≤
Arsenic
≤
0.05
%
0.001
%
≤
Calcium
≤
0.01
%
0
⁢
%
≤
Copper
≤
1
⁢
%
0
⁢
%
≤
Nickel
≤
1
⁢
%
0
⁢
%
≤
Boron
≤
0.05
%
0
⁢
%
≤
Lead
≤
0.2
%
0
⁢
%
≤
Tin
≤
0.2
%
0
⁢
%
≤
Antimony
≤
0.2
%
a remainder of the composition being composed of iron and unavoidable impurities caused by processing,
a microstructure of the steel sheet being made of ferrite and comprising in area fraction, 80% to 100% recrystallized microstructure, 0% to 20% non-recrystallized microstructure wherein an average grain size of recrystallized microstructure is from 20 microns to 110 microns and having a percentage of eddy current losses in total iron losses, measured at 1 T and 400 Hz according to IEC 60404-2 standards, less than 25% when calculated in accordance of Bertotti method and simultaneously having a magnetic polarization at 5000 A/m (J50) from 1.625 T to 1.690 T.

### Claim 2 (depends on 1)

The non-oriented electrical steel sheet as recited in claim 1 wherein the composition includes 0.002% to 0.007% of Carbon.

### Claim 3 (depends on 1)

The non-oriented electrical steel sheet as recited in claim 1 wherein the composition includes 0.85% to 1.1% of Aluminum.

### Claim 4 (depends on 1)

The non-oriented electrical steel sheet as recited in claim 1 wherein the composition includes 0.16% to 0.24% of Manganese.

### Claim 5 (depends on 1)

The non-oriented electrical steel sheet as recited in claim 1 wherein the amount of non-recrystallized microstructure is from 0% to 10%.

### Claim 6 (depends on 1)

The non-oriented electrical steel sheet as recited in claim 1 wherein the amount of recrystallized microstructure is from 90% to 100%.

### Claim 7 (depends on 1)

The non-oriented electrical steel sheet as recited in claim 1 wherein the steel sheet has an ultimate tensile strength of at least 540 MPa in both a transversal direction as well as a rolling direction.

### Claim 8 (depends on 1)

The non-oriented electrical steel sheet as recited in claim 1 wherein the steel sheet has a yield strength from 430 MPa or more in both a transversal direction as well as a rolling direction.

### Claim 9 (depends on 1)

The non-oriented electrical steel sheet as recited in claim 1 wherein the steel sheet has a total elongation of at least 14% in both transversal direction as well as a rolling direction.

### Claim 10 (depends on 1)

A method of production of a non-oriented electrical steel sheet as recited in claim 1 comprising the following successive steps:
providing a semi-finished product having the composition;
reheating the semi-finished product to a temperature from 1100° C. to 1250° C.;
rolling the semi-finished product wherein the hot rolling finishing temperature is from 840° C. to 900° C. to obtain a hot rolled steel sheet;
cooling the hot rolled sheet immediately after the finishing of hot rolling;
then cooling the hot rolled steel sheet from the finishing of hot rolling to a coiling temperature range which is from 540° C. to 640° C. at a cooling rate of at least 10° C./s;
thereafter coiling the hot rolled steel sheet in the coiling temperature range from 540° C. to 640° C.;
optionally performing scale removal process on the hot rolled steel sheet;
optionally hot band annealing is performed on the hot rolled steel sheet from 650° C. to 1100° C. during 10 seconds to 96 hours;
optionally performing scale removal process on the hot rolled steel sheet;
cold rolling the hot rolled steel sheet with a reduction rate from 50% to 95% to obtain a cold rolled steel sheet;
thereafter annealing the cold rolled steel sheet wherein the heating for annealing starts from room temperature to an annealing temperature range Tsoak which is from 900° C. to 1000° C., with a heating rate HR1 of at least 1° C./s;
then perform annealing at annealing temperature during 10 to 5000 seconds;
then cooling the cold rolled steel sheet starting from the annealing temperature to a temperature T1 from 300° C. to 20° C., with a cooling rate CR1 from 1° C./s to 150° C./s; and
then cooling to room temperature to obtain a non-oriented electrical steel sheet.

### Claim 11 (depends on 10)

The method as recited in claim 10 wherein the Tsoak temperature for annealing is from 900° C. to 980° C.

### Claim 12 (depends on 10)

The method as recited in claim 10 wherein temperature T1 is from 200° C. to 20° C.

### Claim 13 (depends on 10)

The method as recited in claim 10 wherein the cooling rate CR1 is from 3° C./s to 120° C./s.