# US 2025/0210700 A1 · All-solid secondary battery

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2025/0210700 A1
- Document ID: US20250210700A1
- Status: Published application
- Kind: A1
- Application number: 19/074,988
- Filed: 2025-03-10
- Published: 2025-06-26
- Earliest claimed: 2021-03-24
- Assignees: Samsung Electronics Co., Ltd.
- Applicants: Samsung Electronics Co., Ltd.
- Inventors: Nobuyoshi YASHIRO; Shoichi SUGATA
- Web page: https://patentgrep.com/patent/US20250210700A1

## CPC

- H01M 10/0562: Solid materials
- H01M 4/131: Electrodes based on mixed oxides or hydroxides, or on mixtures of oxides or hydroxides, e.g. LiCoOx
- H01M 4/133: Electrodes based on carbonaceous material, e.g. graphite-intercalation compounds or CFx
- H01M 4/134: Electrodes based on metals, Si or alloys
- H01M 4/364: {as mixtures}
- H01M 4/366: {as layered products}
- H01M 4/38: of elements or alloys
- H01M 4/382: {Lithium (H01M4/405 takes precedence)}
- H01M 4/386: {Silicon or alloys based on silicon}
- H01M 4/525: of mixed oxides or hydroxides containing iron, cobalt or nickel for inserting or intercalating light metals, e.g. LiNiO2, LiCoO2 or LiCoOxFy
- H01M 4/587: for inserting or intercalating light metals
- H01M 4/621: {Binders}
- H01M 10/0525: Rocking-chair batteries, i.e. batteries with lithium insertion or intercalation in both electrodes; Lithium-ion batteries
- H01M 10/056: characterised by the materials used as electrolytes, e.g. mixed inorganic/organic electrolytes
- H01M 10/0585: of accumulators having only flat construction elements, i.e. flat positive electrodes, flat negative electrodes and flat separators
- H01M 50/431: Inorganic material
- H01M 50/46: Separators, membranes or diaphragms characterised by their combination with electrodes
- H01M 2004/021: {Physical characteristics, e.g. porosity, surface area}
- H01M 2004/027: {Negative electrodes}
- H01M 2004/028: {Positive electrodes}
- H01M 2010/4292: {Aspects relating to capacity ratio of electrodes/electrolyte or anode/cathode}
- H01M 2300/0068: inorganic
- H01M 2300/0071: Oxides
- Y02E 60/10: Energy storage using batteries
- H01M: PROCESSES OR MEANS, e.g. BATTERIES, FOR THE DIRECT CONVERSION OF CHEMICAL ENERGY INTO ELECTRICAL ENERGY
- Y02E: REDUCTION OF GREENHOUSE GAS [GHG] EMISSIONS, RELATED TO ENERGY GENERATION, TRANSMISSION OR DISTRIBUTION

## Abstract

An secondary battery includes a cathode layer, an anode layer having an anode current collector and an anode active material layer on the anode current collector, a lithium metal layer or a lithium alloy layer between the anode current collector and the anode active material layer, wherein the lithium metal layer or the lithium alloy layer has a thickness in a range of about 10 micrometers to about 60 micrometers, and a solid electrolyte layer between the cathode layer and the anode layer, wherein the solid electrolyte is an oxide, phosphate, borate, sulfate, an oxynitride, or a combination thereof.

## Claims

### Claim 1

A secondary battery comprising:
a cathode layer;
an anode layer comprising an anode current collector and a layer comprising an anode active material and a binder on the anode current collector;
a lithium metal layer or a lithium alloy layer between the anode current collector and the anode active material layer, wherein the lithium metal layer or the lithium alloy layer has a thickness in a range of about 10 micrometers to about 60 micrometers; and
a solid electrolyte layer between the cathode layer and the anode layer, wherein the solid electrolyte layer comprises;
Li1+x+yAlxTi2−xSiyP3−yO12 wherein 0<x<2, and 0≤y<3, Pb(Zr1−aTia)O3 wherein 0≤a≤1, Pb1−xLaxZr1−yTiyO3 wherein 0≤x<1, and 0≤y<1, Pb(Mg1/3Nb2/3)O3—PbTiO3, Li3PO4, LixTiy(PO4)3 wherein 0<x<2, and 0<y<3, LixAlyTiz(PO4)3 wherein 0<x<2, 0<y<1, and 0<z<3, Li1+x+y(AlaGa1−a)x(TibGe1−b)2−xSiyP3−yO12 wherein 0≤x≤1, 0≤y≤1, 0≤a≤1, and 0≤b≤1, LixLayTiO3 wherein 0<x<2, and 0<y<3, LiAlO2, a Li2O—Al2O3—SiO2—P2O5—TiO2—GeO2, Li3+xLa3M2O12 wherein M is Te, Nb, Zr, or a combination thereof, and 0≤x≤10, Li7La3Zr2−xTaxO12 wherein 0<x<2, or a combination thereof.

### Claim 2 (depends on 1)

The secondary battery of claim 1, wherein the anode active material that forms an alloy or a compound with lithium comprises an alloy-forming element comprising gold, platinum, palladium, silicon, silver, aluminum, bismuth, tin, zinc, or a combination thereof.

### Claim 3 (depends on 1)

The secondary battery of claim 1, wherein the anode active material is in the form of particles, and wherein the particles have a particle diameter in a range of about 20 nanometers to about 4 micrometers.

### Claim 4 (depends on 3)

The secondary battery of claim 3, further comprising a conductive coating layer disposed on a surface of the particles, wherein a thickness of the conductive coating layer is in a range of about 1 nanometer to about 10 nanometers.

### Claim 5 (depends on 1)

The secondary battery of claim 1, wherein an amount of the alloy-forming element is in a range of about 8 wt % to about 23 wt %, and an amount of the amorphous carbon is in a range of about 60 wt. % to about 86 wt. %, each based on a weight of the anode active material layer.

### Claim 6 (depends on 1)

The secondary battery of claim 1, wherein an amount of the binder is in a range of about 0.5 parts to about 30 parts by weight based on 100 parts by weight of the anode active material layer.

### Claim 7 (depends on 1)

The secondary battery of claim 1, wherein the cathode layer comprises a cathode active material layer, and the anode layer comprises an anode active material layer,
wherein a ratio of a charge capacity of the cathode active material layer to a charge capacity of the anode active material layer satisfies Expression (1):
0.01
<
b
/
a
<
0.5
(
1
)
wherein in Expression 1, a is a charge capacity of the cathode active material layer and b is a charge capacity of the anode active material layer.

### Claim 8 (depends on 1)

The secondary battery of claim 1, wherein a thickness of the anode active material layer is in a range of about 1 micrometer to about 20 micrometers.

### Claim 9 (depends on 1)

The secondary battery of claim 1, wherein a surface roughness of a surface of the solid electrolyte layer in contact with the anode active material layer is in a range of about 0.05 micrometer Ra to about 0.6 micrometer Ra.

### Claim 10 (depends on 1)

The secondary battery of claim 1, wherein a binding strength between the anode layer and the solid electrolyte layer is in a range of about 14 millinewtons per millimeter to about 100 millinewtons per millimeter.

### Claim 11 (depends on 1)

The secondary battery of claim 1, wherein a film strength of the anode active material layer is in a range of about 16 megapascals to about 85 megapascals.

### Claim 12 (depends on 1)

The secondary battery of claim 1, wherein the solid electrolyte layer is directly on the anode active material layer.

### Claim 13 (depends on 1)

The secondary battery of claim 1, wherein the cathode layer comprises a cathode active material layer,
wherein the cathode active material layer comprises a cathode active material,
wherein the cathode active material comprises a compound selected from the group consisting of lithium cobalt oxide, lithium nickel oxide, lithium nickel cobalt oxide, lithium nickel cobalt aluminum oxide, lithium nickel cobalt manganese oxide, lithium manganate, lithium iron phosphate, nickel sulfide, copper sulfide, lithium sulfide, sulfur, iron oxide, vanadium oxide, and a combination thereof.

### Claim 14 (depends on 13)

The secondary battery of claim 13, wherein the cathode active material comprises a lithium transition metal oxide having a layered structure and represented by one of Formulae 1 to 5:
LiaNixCoyMzO2−bAb Formula 1
wherein, in Formula 1,
1.0≤a≤1.2, 0≤b≤0.2, 0.3≤x<1, 0≤y≤0.3, 0<z≤0.3, and x+y+z=1,
M is selected from the group consisting of manganese, niobium, vanadium, magnesium, gallium, silicon, tungsten, molybdenum, iron, chromium, copper, zinc, titanium, aluminum, and a combination thereof,
A is F, S, Cl, Br, or a combination thereof,
LiNixCoyMnzO2, Formula 2
wherein in Formula 2 x, y, and z are each independently 0.3≤x≤0.95, 0≤y≤0.2, 0<z≤0.2, and x+y+z=1,
LiNixCoyAlzO2 Formula 3
wherein in Formula 3, x, y, and z are each independently 0.3≤x≤0.95, 0≤y≤0.2, 0<z≤0.2, and x+y+z=1,
LiNixCoyMnvAlwO2 Formula 4
wherein, in Formula 4, 0.3≤x≤0.95, 0≤y≤0.2, 0<v≤0.2, 0<w≤0.2, and x+y+v+w=1,
LiaCoxMyO2−bAb Formula 5
wherein, in Formula 5,
1.0≤a≤1.2, 0≤b≤0.2, 0.9≤x≤1, 0≤y≤0.1, and x+y=1,
M is selected from the group consisting of manganese, niobium, vanadium, magnesium, gallium, silicon, tungsten, molybdenum, iron, chromium, copper, zinc, titanium, aluminum, and a combination thereof, and
A is F, S, Cl, Br, or a combination thereof.

### Claim 15 (depends on 1)

The secondary battery of claim 1, wherein the cathode layer comprises a cathode active material layer, and wherein the cathode active material layer further comprises a second solid electrolyte.

### Claim 16 (depends on 15)

The secondary battery of claim 15, wherein the second solid electrolyte comprises an oxide solid electrolyte or a sulfide solid electrolyte, or a combination thereof.

### Claim 17 (depends on 1)

The secondary battery of claim 1, wherein anode current collector is in a plate form or a foil form.

### Claim 18

A method of preparing a secondary battery, the method comprising:
providing a solid electrolyte layer on a substrate;
acid-treating the solid electrolyte layer to provide an acid-treated solid electrolyte layer; and
stacking the acid-treated solid electrolyte layer between a cathode layer and an anode layer, such that a binding strength between the solid electrolyte layer and the anode layer is in a range of about 14 millinewtons per millimeter to about 100 millinewtons per millimeter.

### Claim 19 (depends on 18)

The method of claim 18, further comprising polishing a surface of the solid electrolyte layer.

### Claim 20 (depends on 18)

The method of claim 18, wherein the anode layer comprises an anode current collector; and an anode active material layer stacked on the anode current collector,
wherein a film strength of the anode active material layer is in a range of about 16 megapascals to about 85 megapascals.