# US 2025/0154617 A1 · Steel plate for advanced nuclear power unit reactor core shell cylinder and manufacturing method for steel plate

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2025/0154617 A1
- Document ID: US20250154617A1
- Status: Published application
- Kind: A1
- Application number: 18/838,924
- Filed: 2022-05-10
- Published: 2025-05-15
- Earliest claimed: 2022-05-06
- Assignees: Angang Steel Company Limited
- Applicants: Angang Steel Company Limited
- Inventors: Chu WANG; Yong WANG; Jiangtao DUAN; Fangfang AI; Jingong CONG; Xinling LI; Diandong SUN; Yupu BAI; Enjun FANG
- Web page: https://patentgrep.com/patent/US20250154617A1

## CPC

- C21D 9/08: for tubular bodies or pipes
- C21C 7/0075: {Treating in a ladle furnace, e.g. up-/reheating of molten steel within the ladle}
- C21C 7/064: Dephosphorising; Desulfurising
- C21C 7/068: Decarburising
- C21C 7/10: Handling in a vacuum
- C21D 1/18: Hardening (C21D1/02 takes precedence); Quenching with or without subsequent tempering (quenching devices C21D1/62)
- C21D 1/28: Normalising
- C21D 6/004: {containing Cr and Ni}
- C21D 6/005: {containing Mn}
- C21D 6/008: {containing Si}
- C21D 8/0226: {Hot rolling}
- C21D 8/0263: {following hot rolling}
- C21D 8/10: during manufacturing of tubular bodies
- C21D 9/46: for sheet metals
- C22B 9/18: Electroslag remelting {(electroslag casting B22D23/10)}
- C22C 33/04: by melting
- C22C 38/001: {containing N}
- C22C 38/002: {containing In, Mg, or other elements not provided for in one single group C22C38/001 - C22C38/60}
- C22C 38/008: {containing tin}
- C22C 38/02: containing silicon
- C22C 38/04: containing manganese
- C22C 38/06: containing aluminium
- C22C 38/44: with molybdenum or tungsten
- C22C 38/46: with vanadium
- C22C 38/48: with niobium or tantalum
- C22C 38/50: with titanium or zirconium
- C21D 2211/002: Bainite
- C21D 2211/005: Ferrite
- C21D 2211/008: Martensite
- Y02E 30/30: Nuclear fission reactors
- C21D: MODIFYING THE PHYSICAL STRUCTURE OF FERROUS METALS; GENERAL DEVICES FOR HEAT TREATMENT OF FERROUS OR NON-FERROUS METALS OR ALLOYS; MAKING METAL MALLEABLE, e.g. BY DECARBURISATION OR TEMPERING (surface treatment of metallic material involving at least one process provided for in class C23 and at least one process covered by this subclass C23F17/00; unidirectional solidification of eutectic materials or unidirectional demixing of eutectoid materials C30B)
- C21C: PROCESSING OF PIG-IRON, e.g. REFINING, MANUFACTURE OF WROUGHT-IRON OR STEEL; TREATMENT IN MOLTEN STATE OF FERROUS ALLOYS
- C22B: PRODUCTION AND REFINING OF METALS (electrolytic C25); PRETREATMENT OF RAW MATERIALS
- C22C: ALLOYS (treatment of alloys C21D, C22F)
- Y02E: REDUCTION OF GREENHOUSE GAS [GHG] EMISSIONS, RELATED TO ENERGY GENERATION, TRANSMISSION OR DISTRIBUTION

## Abstract

A steel plate for an advanced nuclear power unit reactor core shell cylinder and a manufacturing method for the steel plate. The steel plate comprises the following components in percentage by mass: 0.10%-0.14% of C, 0.20%-0.30% of Si, 0.30%-0.60% of Mn, P≤0.006%, S≤0.002%, 1.65%-1.95% of Cr, 0.80%-1.20% of Mo, 0.80%-1.20% of Ni, 0.04%-0.08% of Nb, 0.10%-0.20% of V, 0%-0.03% of Ti, 0%-0.02% of Alt, 0.001%-0.004% of Ca, 0.01%-0.03% of N, Sn≤0.001%, H≤0.0001%, and 0≤0.0020%, and the remainder being Fe and inevitable inclusions, and an anti-high-temperature tempering embrittlement coefficient J=(Si+Mn)×(P+Sn)×104≤50. The steel plate and the manufacturing method therefor can ensure the comprehensive performance requirements of the steel plate for the reactor core shell cylinder.

## Claims

### Claim 1

A steel plate for a reactor core shell cylinder of an advanced nuclear power unit, comprising the following components in percentage by mass: 0.10%-0.14% of C, 0.20%-0.30% of Si, 0.30%-0.60% of Mn, less than or equal to 0.006% of P, less than or equal to 0.002% of S, 1.65%-1.95% of Cr, 0.80%-1.20% of Mo, 0.80%-1.20% of Ni, 0.04%-0.08% of Nb, 0.10%-0.20% of V, 0%-0.03% of Ti, 0%-0.02% of Alt, 0.001%-0.004% of Ca, 0.01%-0.03% of N, less than or equal to 0.001% of Sn, less than or equal to 0.0001% of H, less than or equal to 0.0020% of O, and balance of Fe and inevitable impurities, wherein a high-temperature tempering embrittlement resistance coefficient J is equal to (Si+Mn)×(P+Sn)×104≤50.

### Claim 2 (depends on 1)

The steel plate for a reactor core shell cylinder of an advanced nuclear power unit according to claim 1, wherein a yield strength at normal temperature as-supplied state of the steel plate satisfies 500 MPa≤Rel≤520 MPa, a tensile strength satisfies 610 MPa≤Rm≤640 MPa, and a tensile strength at 500° C. satisfies 470 MPa≤Rm≤485 MPa.

### Claim 3 (depends on 1)

The steel plate for a reactor core shell cylinder of an advanced nuclear power unit according to claim 1, wherein a tensile strength at 500° C. after post-weld heat treatment at 700° C. for 26 h satisfies 450 MPa≤Rm≤470 MPa, an impact power KV2 at 80° C. is higher than or equal to 420 J, a nil-ductility transition temperature TNDT is lower than or equal to −40° C., a CSR of HIC A solution is 0%, and a fracture toughness KIC satisfies 280 MPa·m1/2≤KIC≤285 MPa·m1/2.

### Claim 4 (depends on 1)

The steel plate for a reactor core shell cylinder of an advanced nuclear power unit according to claim 1, wherein a structure containing 10-15% undissolved ferrite and tempered bainite is obtained, wherein the bainite structure comprises an alloy carbide with a dispersed precipitates M23C6 structure, of which M is a combination of Fe, Mn, Cr and Mo.

### Claim 5 (depends on 1)

The steel plate for a reactor core shell cylinder of an advanced nuclear power unit according to claim 1, wherein Mo/Si is 2.80-5.50, and (Cr+Mn)/Mo is 1.65-2.90.

### Claim 6 (depends on 1)

A method for manufacturing the steel plate for a reactor core shell cylinder of an advanced nuclear power unit according to claim 1, comprising a smelting process, a casting process, an electroslag remelting process, a heating process, a rolling process, and a heat treatment process, with the following steps of:
1) smelting process: performing deep desulfurization treatment to liquid steel in a LF refining furnace, controlling a sulfur content to be less than or equal to 0.002%, while feeding CaSi wires into the steel for calcium treatment;
a thickness of a generated slag layer is 60-90 mm;
performing degassing in a RH furnace with a net cycle time of 10-15 min and a sedation time before casting of 3-5 min;
2) casting process: casting, with a superheat degree of 20-30° C., the smelted liquid steel by a conticaster at a constant speed after breaking vacuum to obtain a casting blank; stacking the casting blank coming off a production line for slow cooling, and then destacking it at a preset temperature;
3) electroslag remelting process: rolling with a 300-400 mm remelted electroslag steel ingot to obtain a steel plate for an shell cylinder with a specification of smaller than or equal to 65 mm; stacking the remelted electroslag steel ingot for slow cooling after demoulding, and then destacking it at a preset temperature;
4) heating process: controlling a temperature for heating the remelted electroslag steel ingot to be 1180-1250° C., a heating time to be 6-8 h, and a soaking time to be 0.5-1.0 h;
5) rolling process: rolling with an initial rolling temperature of 1050-1150° C. in a recrystallization zone, a single-pass deformation rate of 10-14% in the recrystallization zone, a reduction rate of each of the first three passes of ≥12%, a total deformation rate of ≥50%, and a thickness of an intermediate billet of 2.0-4.0 times that of a finished steel plate, and rolling with an initial rolling temperature of 850-900° C. in a non-recrystallization zone, a finishing rolling temperature of 820-850° C. in the non-recrystallization zone, and a cumulative deformation rate of ≥50% in the non-recrystallization zone, wherein a thickness of the finished product after rolling is 40-65 mm;
6) heat treatment process: performing high-temperature normalizing to the finished product at a temperature of Ac3+(80-130) ° C., with a holding time of 0.5-1.0 min/mm, and then performing air cooling to room temperature;
performing intercritical hardening to the finished product at a temperature of 800-850° C., with a holding time of 1.0-1.5 min/mm, a cooling rate of 5-10° C./S, a self-tempering temperature of 350-450° C., and then performing air cooling to room temperature; and
performing high-temperature tempering heat treatment.

### Claim 7 (depends on 6)

The method according to claim 6, wherein in the smelting process, liquid steel is smelted in a converter, and melted iron and scrap steel are used as raw materials, wherein a content of the melted iron is controlled to be 70-80%; and
dephosphorization and decarburization are separately performed in the converter, wherein a time for dephosphorization oxygen blowing ranges from 7 min to 10 min, a time for decarburization oxygen blowing ranges from 8 min to 12 min, and a mass fraction of phosphorus is ultimately reduced to less than or equal to 0.006%.

### Claim 8 (depends on 6)

The method according to claim 6, wherein during the calcium treatment of the smelting process, a wire feeding speed is 200-350 m/min, and a wire feeding depth is 1.0-2.0 m below the slag layer.

### Claim 9 (depends on 6)

The method according to claim 6, wherein in the casting process, a stacking time for slow cooling is 36-54 h, and a destacking temperature is below 300° C.; and
in the electroslag remelting process, a stacking time for slow cooling after the electroslag steel ingots are demoulded is 48-72 h, and the destacking is performed below 400° C. for air cooling.

### Claim 10 (depends on 6)

The method according to claim 6, wherein process parameters of the high-temperature tempering heat treatment are as follows: a tempering temperature of 710-730° C. and a holding time of 60 min+2.0-4.0 min/mm.