# US 2025/0153234 A1 · Hot press-formed part and manufacturing method thereof

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2025/0153234 A1
- Document ID: US20250153234A1
- Status: Published application
- Kind: A1
- Application number: 18/838,858
- Filed: 2023-04-26
- Published: 2025-05-15
- Earliest claimed: 2022-05-06
- Assignees: Posco
- Applicants: Posco Co., Ltd
- Inventors: Sang-Heon Kim; Jin-Keun Oh; Seong-Woo Kim; Sea-Woong Lee; Hyeon-Seok Hwang; Kkoch-Nim Oh
- Web page: https://patentgrep.com/patent/US20250153234A1

## CPC

- B21D 22/022: {by heating the blank or stamping associated with heat treatment (C21D takes precedence)}
- C22C 38/12: containing tungsten, tantalum, molybdenum, vanadium, or niobium
- B32B 15/012: {one layer being formed of an iron alloy or steel, another layer being formed of aluminium or an aluminium alloy}
- C21D 1/18: Hardening (C21D1/02 takes precedence); Quenching with or without subsequent tempering (quenching devices C21D1/62)
- C21D 1/26: Methods of annealing
- C21D 1/673: for die quenching
- C21D 6/001: {containing Ni (C21D6/004 takes precedence)}
- C21D 6/005: {containing Mn}
- C21D 6/008: {containing Si}
- C21D 7/13: by hot working
- C21D 8/02: during manufacturing of plates or strips (C21D8/12 takes precedence)
- C21D 8/0226: {Hot rolling}
- C21D 8/0263: {following hot rolling}
- C21D 8/0278: involving a particular surface treatment (C21D8/0294 takes precedence)
- C21D 9/0068: {for particular articles not mentioned below}
- C21D 9/46: for sheet metals
- C21D 9/48: deep-drawing sheets
- C22C 38/001: {containing N}
- C22C 38/002: {containing In, Mg, or other elements not provided for in one single group C22C38/001 - C22C38/60}
- C22C 38/005: {containing rare earths, i.e. Sc, Y, Lanthanides}
- C22C 38/008: {containing tin}
- C22C 38/02: containing silicon
- C22C 38/04: containing manganese
- C22C 38/06: containing aluminium
- C22C 38/08: containing nickel {(C22C38/105 takes precedence)}
- C22C 38/14: containing titanium or zirconium
- C22C 38/16: containing copper
- C22C 38/60: containing lead, selenium, tellurium, or antimony, or more than 0.04% by weight of sulfur
- C23C 2/022: {by heating}
- C23C 2/024: {by cleaning or etching}
- C23C 2/12: Aluminium or alloys based thereon
- C23C 2/28: Thermal after-treatment, e.g. treatment in oil bath
- C23F 17/00: Multi-step processes for surface treatment of metallic material involving at least one process provided for in class C23 and at least one process covered by subclass C21D or C22F or class C25 (coating for obtaining at least two superposed coatings either by methods not provided for in a single one of main groups C23C2/00 - C23C26/00, or by combinations of methods providedfor in subclasses C23C and C25D, C23C28/00)
- C23G 1/08: Iron or steel
- C23G 1/081: {solutions containing H2SO4}
- C21D 2211/002: Bainite
- C21D 2211/008: Martensite
- B21D: WORKING OR PROCESSING OF SHEET METAL OR METAL TUBES, RODS OR PROFILES WITHOUT ESSENTIALLY REMOVING MATERIAL; PUNCHING METAL (working or processing of wire B21F)
- C22C: ALLOYS (treatment of alloys C21D, C22F)
- B32B: LAYERED PRODUCTS, i.e. PRODUCTS BUILT-UP OF STRATA OF FLAT OR NON-FLAT, e.g. CELLULAR OR HONEYCOMB, FORM
- C21D: MODIFYING THE PHYSICAL STRUCTURE OF FERROUS METALS; GENERAL DEVICES FOR HEAT TREATMENT OF FERROUS OR NON-FERROUS METALS OR ALLOYS; MAKING METAL MALLEABLE, e.g. BY DECARBURISATION OR TEMPERING (surface treatment of metallic material involving at least one process provided for in class C23 and at least one process covered by this subclass C23F17/00; unidirectional solidification of eutectic materials or unidirectional demixing of eutectoid materials C30B)
- C23C: COATING METALLIC MATERIAL; COATING MATERIAL WITH METALLIC MATERIAL; SURFACE TREATMENT OF METALLIC MATERIAL BY DIFFUSION INTO THE SURFACE, BY CHEMICAL CONVERSION OR SUBSTITUTION; COATING BY VACUUM EVAPORATION, BY SPUTTERING, BY ION IMPLANTATION OR BY CHEMICAL VAPOUR DEPOSITION, IN GENERAL (making metal-coated products by extrusion B21C23/22; covering with metal by connecting pre-existing layers to articles, see the relevant places, e.g. B21D39/00, B23K; metallising of glass C03C; metallising mortars, concrete, artificial stone, ceramics or natural stone C04B41/00; enamelling of, or applying a vitreous layer to, metals C23D; treating metal surfaces or coating of metals by electrolysis or electrophoresis C25D; single-crystal film growth C30B; by metallising textiles D06M11/83; decorating textiles by locally metallising D06Q1/04)
- C23F: NON-MECHANICAL REMOVAL OF METALLIC MATERIAL FROM SURFACE (working metal by laser beams B23K26/00; desurfacing by applying flames B23K7/00; working of metal by electro-erosion B23H; producing decorative effects by removing surface material, e.g. by engraving, by etching, B44C1/22; electrolytic etching or polishing C25F); INHIBITING CORROSION OF METALLIC MATERIAL OR INCRUSTATION IN GENERAL; MULTI-STEP PROCESSES FOR SURFACE TREATMENT OF METALLIC MATERIAL INVOLVING AT LEAST ONE PROCESS PROVIDED FOR IN CLASS C23 AND AT LEAST ONE PROCESS COVERED BY SUBCLASS C21D OR C22F OR CLASS C25
- C23G: CLEANING OR DE-GREASING OF METALLIC MATERIAL BY CHEMICAL METHODS OTHER THAN ELECTROLYSIS

## Abstract

Provided are a hot press-formed part and a manufacturing method thereof, the hot press-formed part comprising: a base steel sheet; and a plating layer provided on at least one surface of the base steel sheet, wherein the plating layer includes an average number of Kirkendall voids per unit area in a specific range, in an area within 20 μm from the interface between the base steel sheet and the plating layer.

## Claims

### Claim 1

A hot press-formed part, comprising:
a base steel sheet; and
a plating layer on at least one surface of the base steel sheet,
wherein the plating layer comprises an average number per unit area of Kirkendall voids having a long diameter of 0.5 μm-5 μm present in a region within 20 μm from an interface between the base steel sheet and the plating layer satisfies 8/1000 μm2-100/1000 μm2.

### Claim 2 (depends on 1)

The hot press-formed part of claim 1, wherein the average number per unit area of Kirkendall voids satisfies 10/1000 μm2-95/1000 μm2.

### Claim 3 (depends on 1)

The hot press-formed part of claim 1, wherein the average number per unit area of Kirkendall voids satisfies 18/1000 μm2-92/1000 μm2.

### Claim 4 (depends on 1)

The hot press-formed part of claim 1, wherein the base steel sheet comprises, by weight %, C: 0.02-0.5%, Si: 0.001-2%, Al: 0.001-1%, Mn: 0.1-4%, P: 0.05% or lower (excluding 0%), S: 0.02% or lower (excluding 0%), N: 0.02% or lower (excluding 0%), Ti: 0.1% or lower (including 0%), B: 0.0001-0.01%, Mo: 1.00% or lower (including 0%), V: 1.00% or lower (including 0%), Ca: 0.01% or lower (including 0%), Nb: 0.1% or lower (including 0%), W: 1% or lower (including 0%), REM: 0.3% or lower (including 0%), and a balance of Fe and inevitable impurities.

### Claim 5 (depends on 1)

The hot press-formed part of claim 1, wherein the base steel sheet comprises 0.005-1 weight % of one or more group 1 elements selected from a group consisting of Sb, Sn, As, Bi, Cu and Ni.

### Claim 6 (depends on 1)

The hot press-formed part of claim 1,
wherein the base steel sheet comprises one or more group 1 elements selected from a group consisting of Sb, Sn, As, Bi, Cu and Ni,
wherein the base steel sheet comprises 0.005-0.1% of each of one or more elements selected from a group consisting of Sb, Sn, As and Bi among the group 1 elements, and
wherein the base steel sheet comprises 0.05-1% of each of one or more elements selected from a group consisting of Cu and Ni among the group 1 elements.

### Claim 7 (depends on 1)

The hot press-formed part of claim 1,
wherein the base steel sheet further comprises one or more group 1 elements selected from a group consisting of Sn, As, Bi, Cu and Ni, and satisfies relational expression 1 as below:
[
Relational
⁢
expression
⁢
1
]
X
max
X
c
⁢
o
⁢
a
⁢
t
≥
1
.
5
where Xcoat indicates an average X content in the plating layer, and a unit thereof is weight %, Xmax indicates a maximum value of an X content in the plating layer, and a unit thereof is weight %, and X indicates one or more group 1 elements selected from a group consisting of Sb, Sn, As, Bi, Cu and Ni.

### Claim 8 (depends on 1)

The hot press-formed part of claim 1, wherein the plating layer comprises an average number per unit area of Kirkendall voids having a long diameter of 2 μm to 6 μm present in a region within 20 μm from an interface between the base steel sheet and the plating layer satisfies 10/1000 μm2 to 100/1000 μm2.

### Claim 9

A method of manufacturing a hot forming part, the method comprising:
reheating a steel slab comprising, by weight %, C: 0.02-0.5%, Si: 0.001-2%, Al: 0.001-1%, Mn: 0.1-4%, P: 0.05% or lower (excluding 0%), S: 0.02% or lower (excluding 0%), N: 0.02% or lower (excluding 0%), Ti: 0.1% or lower (including 0%), B: 0.0001-0.01%, Mo: 1.00% or lower (including 0%), V: 1.00% or lower (including 0%), Ca: 0.01% or lower (including 0%), Nb: 0.1% or lower (including 0%), W: 1% or lower (including 0%), REM: 0.3% or lower (including 0%), and a balance of Fe and inevitable impurities, at 1050-1300° C.;
obtaining a hot-rolled steel sheet by finish-rolling the reheated steel slab at 800-950° C.;
coiling the hot-rolled steel sheet at 500-700° C.;
pickling the coiled hot-rolled steel sheet such that a product of acid concentration and pickling time is 800-10,000 g/L s;
continuous annealing the pickled steel sheet by controlling an average temperature increase rate for each zone to satisfy equations 1 to 3 as below;
plating the continuously annealed steel sheet by immersing the steel sheet in a plating bath comprising aluminum or aluminum alloy; and
heat-treating the plated steel sheet at Ac3-950° C. for 1-1000 seconds and hot press-forming the steel sheet:
[
Equation
⁢
1
]
1.5
°
⁢
C
.
/
⁢
s
≤
average
⁢
temperature
⁢
increase
⁢
rate
⁢
in
⁢
zone
⁢
1
⁢
(
°
⁢
C
.
/
⁢
s
)
≤
10.
°
⁢
C
.
/
⁢
s
[
Equation
⁢
2
]
0.5
°
⁢
C
.
/
⁢
s
≤
average
⁢
temperature
⁢
increase
⁢
rate
⁢
in
⁢
zone
⁢
2
⁢
(
°
⁢
C
.
/
⁢
s
)
≤
1.
°
⁢
C
.
/
⁢
s
[
Equation
⁢
3
]
0.01
°
⁢
C
.
/
⁢
s
≤
average
⁢
temperature
⁢
increase
⁢
rate
⁢
in
⁢
zone
⁢
3
⁢
(
°
⁢
C
.
/
⁢
s
)
≤
0.4
°
⁢
C
.
/
⁢
s
where zone 1 refers to a section until a surface temperature of the steel sheet reaches 500° C., zone 2 refers to a section until a surface temperature of the steel sheet reaches 500° C. to 700° C., and zone 3 refers to a section until a surface temperature of the steel sheet reaches a maximum temperature.

### Claim 10

A hot press-formed part, comprising:
a base steel sheet; and
a plating layer on at least one surface of the base steel sheet,
wherein relational expression 2-1 as below is satisfied:
[
Relational
⁢
expression
⁢
2
-
1
]
9
.
5
≤
D
B
⁢
2
/
D
A
⁢
2
≤
11.
where DB2 indicates an absolute value of DFe/DAl in a region in which an atomic content ratio of aluminum (Al) in the hot press-formed part is 0.25-0.45, DA2 indicates an absolute value of DFe/DAl in a region in which an atomic content ratio of aluminum (Al) in the hot press-formed part is 0.25-0.45, and in this case, DFe indicates diffusivity of iron (Fe), and DAl indicates diffusivity of aluminum (Al).

### Claim 11 (depends on 10)

The hot press-formed part of claim 10, wherein a microstructure of the base steel sheet comprises one or more structures selected from a group consisting of martensite and bainite.

### Claim 12 (depends on 10)

The hot press-formed part of claim 10, wherein an average number per unit area of Kirkendall voids having a diameter of 0.5 μm-5 μm present in a region within 20 μm in a direction of the plating layer side from an interfacial surface between the base steel sheet and the plating layer, satisfies 7/1000 μm2-100/1000 μm2.

### Claim 13 (depends on 12)

The hot press-formed part of claim 12, wherein an average number per unit area of the Kirkendall void satisfies 10/1000 μm2-95/1000 μm2.

### Claim 14 (depends on 12)

The hot press-formed part of claim 12, wherein an average number per unit area of the Kirkendall void satisfies 18/1000 μm2-92/1000 μm2.

### Claim 15 (depends on 10)

The hot press-formed part of claim 10, wherein the base steel sheet comprises, by weight %, C: 0.02-0.5%, Si: 0.001-2%, Al: 0.001-1%, Mn: 0.1-4%, P: 0.05% or lower (excluding 0%), S: 0.02% or lower (excluding 0%), N: 0.02% or lower (excluding 0%), Ti: 0.1% or lower (including 0%), B: 0.0001-0.01%, Mo: 1.00% or lower (including 0%), V: 1.00% or lower (including 0%), Ca: 0.01% or lower (including 0%), Nb: 0.1% or lower (including 0%), W: 1% or lower (including 0%), REM: 0.3% or lower (including 0%), and a balance of Fe and inevitable impurities.

### Claim 16 (depends on 10)

The hot press-formed part of claim 10, wherein the base steel sheet independently comprises 0.005 weight %-1 weight % of one or more group 1 elements selected from a group consisting of Sb, Sn, As, Bi, Cu and Ni.

### Claim 17 (depends on 10)

The hot press-formed part of claim 10,
wherein the base steel sheet comprises one or more group 1 elements selected from a group consisting of Sb, Sn, As, Bi, Cu and Ni,
wherein the base steel sheet comprises 0.005-0.1% of each of one or more elements selected from a group consisting of Sb, Sn, As and Bi among the group 1 elements independently, and
wherein the base steel sheet comprises 0.005-1% of each of one or more elements selected from a group consisting of Cu and Ni among the group 1 elements independently.

### Claim 18 (depends on 10)

The hot press-formed part of claim 10,
wherein the base steel sheet further comprises one or more group 1 elements selected from a group consisting of Sn, As, Bi, Cu and Ni, and satisfies relational expression 2-2 as below:
[
Relational
⁢
expression
⁢
2
-
2
]
X
max
X
c
⁢
o
⁢
a
⁢
t
≥
1.5
.
where Xcoat indicates an average X content in the plating layer, and a unit thereof is weight %, Xmax indicates a maximum value of an X content in the plating layer, and a unit thereof is weight %, and X indicates one or more group 1 elements selected from a group consisting of Sb, Sn, As, Bi, Cu and Ni.

### Claim 19 (depends on 10)

The hot press-formed part of claim 10, wherein, in the plating layer, an average number per unit area of Kirkendall voids having a diameter of 2 μm-6 μm present in a region within 20 μm in a direction of the plating layer side from an interface between the base steel sheet and the plating layer, satisfies 10/1000 μm2-100/1000 μm2.

### Claim 20

(canceled)