# US 2025/0146098 A1 · Austenitic stainless steel and method of manufacturing austenitic stainless steel

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2025/0146098 A1
- Document ID: US20250146098A1
- Status: Published application
- Kind: A1
- Application number: 18/836,837
- Filed: 2023-02-08
- Published: 2025-05-08
- Earliest claimed: 2022-03-17
- Assignees: Nippon Steel Corporation
- Applicants: Nippon Steel Corporation
- Inventors: Kana JOTOKU; Takahiro OSUKI; Tsuyoshi KAWANISHI
- Web page: https://patentgrep.com/patent/US20250146098A1

## CPC

- C21D 9/525: {for wire, for rods (C21D9/54 takes precedence)}
- C22C 38/004: {Very low carbon steels, i.e. having a carbon content of less than 0,01%}
- C21D 1/26: Methods of annealing
- C21D 6/004: {containing Cr and Ni}
- C21D 6/005: {containing Mn}
- C21D 6/007: {containing Co}
- C21D 6/008: {containing Si}
- C21D 7/10: of the whole cross-section, e.g. of concrete reinforcing bars
- C21D 8/00: Modifying the physical properties of ferrous metals or ferrous alloys by deformation combined with, or followed by, heat treatment (hardening articles or materials formed by forging or rolling with no further heating beyond that required for the formation C21D1/02)
- C21D 8/06: during manufacturing of rods or wires
- C21D 9/0075: {for rods of limited length (of unlimited length C21D9/52)}
- C22C 38/001: {containing N}
- C22C 38/002: {containing In, Mg, or other elements not provided for in one single group C22C38/001 - C22C38/60}
- C22C 38/02: containing silicon
- C22C 38/04: containing manganese
- C22C 38/06: containing aluminium
- C22C 38/42: with copper
- C22C 38/44: with molybdenum or tungsten
- C22C 38/46: with vanadium
- C22C 38/48: with niobium or tantalum
- C22C 38/52: with cobalt
- C22C 38/54: with boron
- C22C 38/58: with more than 1.5% by weight of manganese
- C21D 2211/001: Austenite
- C21D: MODIFYING THE PHYSICAL STRUCTURE OF FERROUS METALS; GENERAL DEVICES FOR HEAT TREATMENT OF FERROUS OR NON-FERROUS METALS OR ALLOYS; MAKING METAL MALLEABLE, e.g. BY DECARBURISATION OR TEMPERING (surface treatment of metallic material involving at least one process provided for in class C23 and at least one process covered by this subclass C23F17/00; unidirectional solidification of eutectic materials or unidirectional demixing of eutectoid materials C30B)
- C22C: ALLOYS (treatment of alloys C21D, C22F)

## Abstract

An austenitic stainless steel with good strength and ductility is provided. An austenitic stainless steel has a chemical composition of, in mass %: 0.005 to 0.060% C; 0.20 to 1.20% Si; 4.0 to 8.0% Mn; 12.0 to 15.0% Ni; 19.0 to 24.0% Cr; 1.0 to 4.0% Mo; 0.05 to 0.40% Nb; 0.05 to 0.40% V; 0.20 to 0.50% N; up to 0.050% Al; and other elements, the tensile strength being not lower than 800 MPa, the braking elongation being not lower than 35%, the steel satisfying the following expressions, (1) and (2): (1) 0.7×Nb≤[Nb]≤0.30; and (2) 20×[Nb]/D≥0.050. In expressions (1) and (2), the Nb content in the chemical composition represented in mass %, the amount of Nb determined through analysis of an electrolytic extraction residue represented in mass %, and the crystal grain size represented in μm are substituted for “Nb”, “[Nb]”, and “D”, respectively.

## Claims

### Claim 1

An austenitic stainless steel having a chemical composition of, in mass %:
0.005 to 0.060% C;
0.20 to 1.20% Si;
4.0 to 8.0% Mn;
12.0 to 15.0% Ni;
19.0 to 24.0% Cr;
1.0 to 4.0% Mo;
0.05 to 0.40% Nb;
0.05 to 0.40% V;
0.20 to 0.50% N;
up to 0.050% Al;
0 to 3.0% Cu;
0 to 0.50% Co;
0 to 0.0050% Ca;
0 to 0.0050% B;
0 to 0.10% W;
0 to 0.10% Ta; and
balance Fe and impurities,
the impurities including:
up to 0.030% P;
up to 0.010% S; and
up to 0.015% O,
a tensile strength being not lower than 800 MPa,
a braking elongation being not lower than 35%,
an amount of Nb determined through analysis of an electrolytic extraction residue satisfying expression (1) below,
the amount of Nb determined through analysis of the electrolytic extraction residue and a crystal grain size satisfying expression (2) below:
0.7
×
Nb
≤
[
Nb
]
≤
0.3
,
(
1
)
and
20
×
[
Nb
]
/
D
≥
0
.
0
⁢
50
,
(
2
)
in expressions (1) and (2), the Nb content in the chemical composition represented in mass %, the amount of Nb determined through analysis of the electrolytic extraction residue represented in mass %, and the crystal grain size represented in μm are substituted for “Nb”, “[Nb]”, and “D”, respectively.

### Claim 2 (depends on 1)

The austenitic stainless steel according to claim 1, wherein the austenitic stainless steel is a solid member.

### Claim 3 (depends on 2)

The austenitic stainless steel according to claim 2, wherein the solid member is a round bar.

### Claim 4 (depends on 3)

The austenitic stainless steel according to claim 3, having an outer diameter not smaller than 25 mm.

### Claim 5 (depends on 1)

The austenitic stainless steel according to claim 1, wherein the chemical composition includes one or more elements selected from the group consisting of, in mass %:
0.01 to 3.0% Cu;
0.01 to 0.50% Co;
0.0001 to 0.0050% Ca;
0.0001 to 0.0050% B;
0.01 to 0.10% W; and
0.001 to 0.10% Ta.

### Claim 6 (depends on 1)

The austenitic stainless steel according to claim 1, used as a material in equipment for storing or transporting high-pressure hydrogen gas or liquid hydrogen.

### Claim 7 (depends on 1)

A method of manufacturing the austenitic stainless steel according to claim 1, comprising:
performing a primary heat treatment on a steel material having said chemical composition at 1180 to 1280° C.;
after the primary heat treatment, performing cold working on the steel material with a reduction in area not lower than 5% and lower than 20%; and,
after the cold working, performing a secondary heat treatment on the steel material at a temperature of 1000 to 1180° C.

### Claim 8 (depends on 7)