# US 2025/0146097 A1 · High-strength hot dip-coated steel strip with plasticity brought about by microstructural transformation and method for production thereof

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2025/0146097 A1
- Document ID: US20250146097A1
- Status: Published application
- Kind: A1
- Application number: 18/835,332
- Filed: 2023-02-01
- Published: 2025-05-08
- Earliest claimed: 2022-02-02
- Applicants: Salzgitter Flachstahl GmbH
- Inventors: Konstantin Molodov; Norbert Kwiaton
- Web page: https://patentgrep.com/patent/US20250146097A1

## CPC

- C21D 9/52: for wires; for strips {; for rods of unlimited length}
- B32B 15/013: {one layer being formed of an iron alloy or steel, another layer being formed of a metal other than iron or aluminium}
- C21D 6/004: {containing Cr and Ni}
- C21D 6/005: {containing Mn}
- C21D 6/008: {containing Si}
- C21D 8/02: during manufacturing of plates or strips (C21D8/12 takes precedence)
- C21D 8/0226: {Hot rolling}
- C21D 8/0236: {Cold rolling}
- C21D 8/0263: {following hot rolling}
- C21D 8/0273: {Final recrystallisation annealing}
- C22C 38/001: {containing N}
- C22C 38/002: {containing In, Mg, or other elements not provided for in one single group C22C38/001 - C22C38/60}
- C22C 38/02: containing silicon
- C22C 38/04: containing manganese
- C22C 38/06: containing aluminium
- C22C 38/26: with niobium or tantalum
- C22C 38/44: with molybdenum or tungsten
- C22C 38/46: with vanadium
- C22C 38/48: with niobium or tantalum
- C22C 38/50: with titanium or zirconium
- C22C 38/54: with boron
- C22C 38/58: with more than 1.5% by weight of manganese
- C23C 2/06: Zinc or cadmium or alloys based thereon
- C23C 2/28: Thermal after-treatment, e.g. treatment in oil bath
- C23C 2/40: Plates; Strips
- B32B 2311/20: Zinc
- C21D 2211/001: Austenite
- C21D 2211/002: Bainite
- C21D 2211/005: Ferrite
- C21D 2211/008: Martensite
- C21D: MODIFYING THE PHYSICAL STRUCTURE OF FERROUS METALS; GENERAL DEVICES FOR HEAT TREATMENT OF FERROUS OR NON-FERROUS METALS OR ALLOYS; MAKING METAL MALLEABLE, e.g. BY DECARBURISATION OR TEMPERING (surface treatment of metallic material involving at least one process provided for in class C23 and at least one process covered by this subclass C23F17/00; unidirectional solidification of eutectic materials or unidirectional demixing of eutectoid materials C30B)
- B32B: LAYERED PRODUCTS, i.e. PRODUCTS BUILT-UP OF STRATA OF FLAT OR NON-FLAT, e.g. CELLULAR OR HONEYCOMB, FORM
- C22C: ALLOYS (treatment of alloys C21D, C22F)
- C23C: COATING METALLIC MATERIAL; COATING MATERIAL WITH METALLIC MATERIAL; SURFACE TREATMENT OF METALLIC MATERIAL BY DIFFUSION INTO THE SURFACE, BY CHEMICAL CONVERSION OR SUBSTITUTION; COATING BY VACUUM EVAPORATION, BY SPUTTERING, BY ION IMPLANTATION OR BY CHEMICAL VAPOUR DEPOSITION, IN GENERAL (making metal-coated products by extrusion B21C23/22; covering with metal by connecting pre-existing layers to articles, see the relevant places, e.g. B21D39/00, B23K; metallising of glass C03C; metallising mortars, concrete, artificial stone, ceramics or natural stone C04B41/00; enamelling of, or applying a vitreous layer to, metals C23D; treating metal surfaces or coating of metals by electrolysis or electrophoresis C25D; single-crystal film growth C30B; by metallising textiles D06M11/83; decorating textiles by locally metallising D06Q1/04)

## Abstract

A method of producing a hot dip-coated high-strength steel strip with plasticity brought about by microstructural transformation starting from producing a hot-rolled steel strip, etching and optionally cold rolling the hot-rolled steel strip to give a cold-rolled steel strip, subsequently continuously annealing in a continuous process of hot dip coating the cold- or hot-rolled steel strip, subsequently cooling the cold- or hot-rolled steel strip to an intermediate temperature, subsequently further cooling the cold- or hot-rolled steel strip from the intermediate temperature to a cooling stop temperature within a temperature range and at an average cooling rate, and then keeping the temperature within a temperature range, then hot dip coating the cold- or hot-rolled steel strip, and cooling the hot dip coated cold- or hot-rolled steel strip at an average cooling rate to ambient temperature. The corresponding hot dip-coated high-strength steel strip thus has plasticity brought about by microstructural transformation.

## Claims

### Claim 1

A method for producing a hot-dip coated high-strength steel strip with plasticity brought about by microstructural transformation, comprising the following steps:
producing a hot-rolled steel strip consisting of the following elements in wt. %:
C: from 0.15 to 0.205,
Mn: from 1.9 to 2.6,
Al: from 0.2 to 0.7,
Si: from 0.5 to 0.9,
Cr: from 0.2 to 0.5,
Nb: from 0.01 to 0.06,
Mo: <0.15,
B: ≤0.001,
P: ≤0.02,
S: ≤0.005,
and optionally one or more of the following elements in wt. %:
Ti: 0.005 to 0.060,
V: 0.001 to 0.060,
N: 0.0001 to 0.016,
Ni: 0.01 to 0.5 and
Cu: 0.01 to 0.3,
with the remainder being iron including typical steel-associated elements, wherein for a value μ=4.5×([Si]+0.9×[Al]+[Cr])+200×[Nb], in which [Si], [Al], [Cr] and [Nb] are the proportions of the corresponding elements in wt. %, 8≤μ≤16;
acid-cleaning and optionally cold-rolling the hot-rolled steel strip to form a cold-rolled steel
subsequently continuously annealing during a continuous hot-dip coating process of the cold- or hot-rolled steel strip at a maximum temperature between 750° C. to 950° C. inclusive for the total duration of 10 s to 1200 s;
subsequently cooling the cold- or hot-rolled steel strip to an intermediate temperature in a temperature range of 620 to 760° C. at an average cooling rate CR1 of up to 10 K/s;
subsequently further cooling the cold- or hot-rolled steel strip from the intermediate temperature to a cooling stop temperature in a temperature range between 200° C. and 450° C. inclusive at an average cooling rate CR2>CR1 and at most 150 K/s and then maintaining the temperature in the temperature range between 200° C. and 450° C. inclusive for 25 to 500 s;
subsequently hot-dip coating the cold- or hot-rolled steel strip at a temperature between 380 and 500° C.; and
subsequently finally cooling the hot-dip coated cold- or hot-rolled steel strip at an average cooling rate of 1 K/s to 50 K/s to ambient temperature.

### Claim 2 (depends on 1)

The method as claimed in claim 1, wherein 10≤μ≤16 applies for the value μ and the expression [Si]+0.9×[Al]<1.2 applies, wherein [Si] and [Al] are the proportions of the corresponding elements in wt. % on the hot-rolled steel strip.

### Claim 3 (depends on 1)

The method as claimed in claim 1, wherein in the hot-rolled steel strip the content of Nb in ppm is >200.

### Claim 4 (depends on 1)

The method as claimed in claim 1 wherein the proportion of Mn on the hot-rolled steel strip is between 1.95 and 2.4 wt. %, and the proportion of C on the hot-rolled steel strip is at least 0.16 wt. %

### Claim 5 (depends on 1)

The method as claimed in claim 1, wherein the sum of the proportions of the elements Cr and Mo on the hot-rolled steel strip in wt. % is less than 0.5 as expressed by [Cr]+[Mo]<0.5.

### Claim 6 (depends on 1)

The method as claimed in claim 1, wherein the intermediate temperature is in a temperature range of 650 to 730° C. and the steel strip has, when this temperature is reached, a microstructure having at least 10 vol. % ferrite.

### Claim 7 (depends on 1)

The method as claimed in claim 1, wherein the cooling stop temperature is ≤400° C., and after the final cooling to ambient temperature more than 8 vol. % austenite is present in the microstructure, wherein the temperature at which the cold- or hot-rolled steel strip is kept prior to the hot-dip coating is ≤400° C.

### Claim 8 (depends on 1)

The method as claimed in claim 1, wherein the hot-dip coated high-strength steel strip has a tensile strength Rm of at least 900 MPa and a uniform elongation Ag of at least 8%.

### Claim 9 (depends on 1)

The method as claimed in claim 1, wherein the hot-dip coated steel strip is subjected to skin pass rolling with a rolling degree of at most 2%, wherein the Rp0.2 elasticity limit increases by at least 20 MPa owing to the skin pass rolling.

### Claim 10 (depends on 1)

The method as claimed in claim 1, wherein in the case of the hot-rolled steel strip the content of Ti is at least 0.005 wt. %, the content of N is at most 0.008 wt. %, the content of Al is at most 0.5 wt. % and TiN and TiAlN particles having a diameter of >0.96 μm are present in total in a surface proportion of at least 1 μm2/mm2 on a measuring surface of at least 100 mm2 in a slab prior to re-heating and on a measuring surface of at least 20 mm2 in the hot-dip coated high-strength steel strip.

### Claim 11

(canceled)

### Claim 12

(canceled)

### Claim 13

(canceled)

### Claim 14

(canceled)

### Claim 15

(canceled)

### Claim 16

A method for producing a hot-dip coated high-strength steel strip with plasticity brought about by microstructural transformation, comprising the following steps:
producing a hot-rolled steel strip from a slab heated to above 1200° C. consisting of the following elements in wt. %:
C: from 0.15 to 0.205,
Mn: from 1.9 to 2.6,
Al: from 0.2 to 0.7,
Si: from 0.5 to 0.9,
Cr: from 0.2 to 0.5,
Nb: from 0.01 to 0.06,
Mo: <0.15,
B: ≤0.001,
P: ≤0.02,
S: ≤0.005,
and optionally one or more of the following elements in wt. %:
Ti: 0.005 to 0.060,
V: 0.001 to 0.060,
N: 0.0001 to 0.016,
Ni: 0.01 to 0.5 and
Cu: 0.01 to 0.3,
with the remainder being iron including typical steel-associated elements, wherein for a value μ=4.5×([Si]+0.9×[Al]+[Cr])+200×[Nb], in which [Si], [Al], [Cr] and [Nb] are the proportions of the corresponding elements in wt. %, 8≤μ≤16;
acid-cleaning and optionally cold-rolling the hot-rolled steel strip to form a cold-rolled steel strip;
subsequently continuously annealing during a continuous hot-dip coating process of the cold- or hot-rolled steel strip at a maximum temperature between 80° and 870° C. for the total duration of 50 s to 650 s;
subsequently cooling the cold- or hot-rolled steel strip to an intermediate temperature in a temperature range of 620 to 760° C. at an average cooling rate CR1 of up to 10 K/s;
subsequently further cooling the cold- or hot-rolled steel strip from the intermediate temperature to a cooling stop temperature in a temperature range between 280° C. and 450° C. inclusive, at an average cooling rate CR2>CR1 and at most 150 K/s and then maintaining the temperature in the temperature range between 280° C. and 450° C. inclusive, for 25 to 500 s;
subsequently hot-dip coating the cold- or hot-rolled steel strip at a temperature between 38° and 500° C.; and
subsequently finally cooling the hot-dip coated cold- or hot-rolled steel strip at an average cooling rate of 1 K/s to 50 K/s to ambient temperature.

### Claim 17 (depends on 16)

The method as claimed in claim 16, wherein 10≤μ≤16 applies for the value μ and the expression [Si]+0.9×[Al]<1.0 applies, wherein [Si] and [Al] are the proportions of the corresponding elements in wt. % on the hot-rolled steel strip, and wherein in the hot-rolled steel strip the content of Nb in ppm is >300.

### Claim 18 (depends on 17)

The method as claimed in claim 17, wherein the proportion of Mn on the hot-rolled steel strip is between 1.95 and 2.4 wt. %, the proportion of C on the hot-rolled steel strip is at least 0.16 wt. %, and the expression (100 [C]+10 [Mn])/(4.5×([Si]+0.9+[Cr])+200×[Nb])<4.5 applies, wherein [Si], [Al], [Cr], [C] and [Mn] are the proportions of the corresponding elements on the hot-rolled steel strip in wt. %, and wherein the sum of the proportions of the elements Cr and Mo on the hot-rolled steel strip in wt. % is less than 0.5 as expressed by [Cr]+[Mo]<0.5, and wherein the intermediate temperature is in a temperature range of 650 to 730° C. and the steel strip has, when this temperature is reached, a microstructure having at least 10 vol. % ferrite.

### Claim 19 (depends on 18)

The method as claimed in claim 18, wherein the cooling stop temperature is ≤350° C., and after the final cooling to ambient temperature more than 8 vol. % austenite is present in the microstructure, wherein the temperature at which the cold- or hot-rolled steel strip is kept prior to the hot-dip coating is ≤350° C., and wherein the hot-dip coated high-strength steel strip has a tensile strength Rm of at least 900 MPa and a uniform elongation Ag of at least 8%.

### Claim 20 (depends on 19)

The method as claimed in claim 19, wherein the hot-dip coated steel strip is subjected to skin pass rolling with a rolling degree of at most 2%, wherein the Rp0.2 elasticity limit increases by at least 20 MPa owing to the skin pass rolling, and wherein in the case of the hot-rolled steel strip the content of Ti is at least 0.005 wt. %, the content of N is at most 0.008 wt. %, the content of Al is at most 0.5 wt. % and TiN and TiAlN particles having a diameter of >0.96 μm are present in total in a surface proportion of at least 1 μm2/mm2 on a measuring surface of at least 100 mm2 in the slab prior to re-heating and on a measuring surface of at least 20 mm2 in the hot-dip coated high-strength steel strip.

### Claim 21 (depends on 1)

A hot-dip coated high-strength steel strip with a plasticity brought about by microstructural transformation produced by a method as claimed in claim 1, consisting of the following elements in wt. %:
C: from 0.15 to 0.205,
Mn: from 1.9 to 2.6,
Al: from 0.2 to 0.7,
Si: from 0.5 to 0.9,
Cr: from 0.2 to 0.5,
Nb: from 0.01 to 0.06,
Mo: <0.15,
B: ≤0.001,
P: ≤0.02,
S: ≤0.005,
and optionally one or more of the following elements in wt. %:
Ti: 0.005 to 0.060,
V: 0.001 to 0.060,
N: 0.0001 to 0.016,
Ni: 0.01 to 0.5 and
Cu: 0.01 to 0.3,
with the remainder being iron including typical steel-associated elements, wherein for a value μ=4.5×([Si]+0.9×[Al]+[Cr])+200×[Nb], in which [Si], [Al], [Cr] and [Nb] are the proportions of the corresponding elements in wt. %, 8≤μ≤16, wherein the steel strip has a product of Rm tensile strength and uniform elongation Ag of greater than 8000 MPa %, in particular greater than 9000 MPa %, and particularly advantageously between 9900 to 13000 MPa %.

### Claim 22 (depends on 21)

The hot-dip coated high-strength steel strip as claimed in claim 21, wherein the steel strip has a product of Rm tensile strength and uniform elongation Ag of between 9900 to 13000 MPa %.

### Claim 23 (depends on 21)

The hot-dip coated high-strength steel strip as claimed in claim 21, wherein the surface proportion of specific Σ3 grain boundaries having a maximum deviation of 10° to the Σ3 orientation relation of 60° <111>, relating to the overall grain boundary surface for large-angle grain boundaries having a disorientation angle >15°, is less than 30%.

### Claim 24 (depends on 21)

The hot-dip coated high-strength steel strip as claimed in claim 21, wherein the steel strip has a yield strength ratio Rp0.2/Rm of <0.87 and a bake-hardening value BH2 of ≥25 MPa.

### Claim 25 (depends on 21)

The hot-dip coated high-strength steel strip as claimed in claim 21, wherein the microstructure of the hot-dip coated high-strength steel strip comprises at least the following components: 8-16 vol. % residual austenite, >10 and <40 vol. % ferrite, at least a sum of 50 vol. % of bainite, tempered martensite and fresh martensite.

### Claim 26 (depends on 25)

The hot-dip coated high-strength steel strip as claimed in claim 25, wherein the microstructure of the hot-dip coated high-strength steep strip has at least two of the following properties:
the proportion of bainite and fresh martensite in vol. % is, in total, greater than the proportion of tempered martensite in vol. %;
with regard to the bainite, the proportion of granular bainite in vol. % is higher than the proportion of lower bainite in vol. %; and
there is a proportion of at least 2 vol. % of fresh martensite in the total microstructure.