# US 2025/0084505 A1 · High strength aluminium alloys containing silicon and copper for use in additive manufacturing and method of using the same

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2025/0084505 A1
- Document ID: US20250084505A1
- Status: Published application
- Kind: A1
- Application number: 18/830,240
- Filed: 2024-09-10
- Published: 2025-03-13
- Earliest claimed: 2023-09-12
- Assignees: Technology Innovation Institute - Sole Proprietorship LLC
- Applicants: Technology Innovation Institute - Sole Proprietorship LLC
- Inventors: Federico Bosio; Giuseppe Del Guercio; Chinmay Phutela; Lewis Kindleyside; Nesma T. Aboulkhair; Rafael Casas
- Web page: https://patentgrep.com/patent/US20250084505A1

## CPC

- C22C 1/0416: {Aluminium-based alloys}
- B22F 1/05: Metallic powder characterised by the size or surface area of the particles
- B22F 1/052: characterised by a mixture of particles of different sizes or by the particle size distribution
- B22F 9/04: starting from solid material, e.g. by crushing, grinding or milling ({C22C1/1084 takes precedence}; crushing, grinding or milling, in general, see the relevant subclasses, e.g. B02C)
- B22F 9/082: {atomising using a fluid (using centrifugal force B22F9/10)}
- B22F 10/28: Powder bed fusion, e.g. selective laser melting [SLM] or electron beam melting [EBM]
- B33Y 10/00: Processes of additive manufacturing
- B33Y 70/00: Materials specially adapted for additive manufacturing
- B33Y 80/00: Products made by additive manufacturing
- C22C 21/02: with silicon as the next major constituent
- B22F 12/17: to heat the build chamber or platform
- B22F 2202/01: Use of vibrations
- B22F 2304/10: Micron size particles, i.e. above 1 micrometer up to 500 micrometer
- B22F 2998/10: Processes characterised by the sequence of their steps
- B22F 2999/00: Aspects linked to processes or compositions used in powder metallurgy
- Y02P 10/25: Process efficiency
- C22C: ALLOYS (treatment of alloys C21D, C22F)
- B22F: WORKING METALLIC POWDER; MANUFACTURE OF ARTICLES FROM METALLIC POWDER; MAKING METALLIC POWDER (making alloys by powder metallurgy C22C); APPARATUS OR DEVICES SPECIALLY ADAPTED FOR METALLIC POWDER
- B33Y: ADDITIVE MANUFACTURING, i.e. MANUFACTURING OF THREE-DIMENSIONAL [3D] OBJECTS BY ADDITIVE DEPOSITION, ADDITIVE AGGLOMERATION OR ADDITIVE LAYERING, e.g. BY 3D PRINTING, STEREOLITHOGRAPHY OR SELECTIVE LASER SINTERING
- Y02P: CLIMATE CHANGE MITIGATION TECHNOLOGIES IN THE PRODUCTION OR PROCESSING OF GOODS

## Abstract

The present disclosure describes an alloy which achieves a level of densification of 99.5% or greater and a method of making the same, wherein the method may include (a) depositing a first layer of a precursor powder including aluminum, silicon, and copper onto a build platform, (b) contacting the first layer of the precursor powder with an energy source to form a solid layer, (c) depositing a subsequent layer of the precursor powder on top of the solid layer, (d) contacting the subsequent layer of the precursor powder with the energy source to fuse the subsequent layer of the precursor powder to the solid layer, thereby forming the three-dimensional article.

## Claims

### Claim 1

A method for forming a three-dimensional article comprising an alloy, the method comprising steps of:
(a) depositing a first layer of a precursor powder onto a build platform, wherein the precursor powder comprises aluminum, silicon, and copper;
(b) contacting the first layer of the precursor powder with an energy source to form a solid layer of the alloy;
(c) depositing a subsequent layer of the precursor powder on top of the solid layer; and
(d) contacting the subsequent layer of the precursor powder with the energy source to fuse the subsequent layer of the precursor powder to the solid layer;
thereby forming the three-dimensional article.

### Claim 2 (depends on 1)

The method of claim 1, wherein the precursor powder comprises greater than or equal to 4 wt. % to less than or equal to 8 wt. % copper.

### Claim 3 (depends on 1)

The method of claim 1, wherein the precursor powder comprises:
greater than or equal to 4 wt. % to less than or equal to 8 wt. % copper, and
greater than or equal to 8 wt. % to less than or equal to 11 wt. % silicon.

### Claim 4 (depends on 1)

The method of claim 1, wherein the precursor powder comprises:
greater than or equal to 4 wt. % to less than or equal to 8 wt. % copper, greater than or equal to 8 wt. % to less than or equal to 11 wt. % silicon, and
greater than or equal to 75 wt. % to less than or equal to 88 wt. % aluminum.

### Claim 5 (depends on 1)

The method of claim 1, wherein the precursor powder comprises:
greater than or equal to 4 wt. % to less than or equal to 8 wt. % copper,
greater than or equal to 8 wt. % to less than or equal to 11 wt. % silicon,
greater than or equal to 0.01 wt. % to less than or equal to 0.8 wt. % iron, and
greater than or equal to 75 wt. % to less than or equal to 88 wt. % aluminum.

### Claim 6 (depends on 1)

The method of claim 1, wherein the precursor powder comprises:
greater than or equal to 4 wt. % to less than or equal to 8 wt. % copper,
greater than or equal to 8 wt. % to less than or equal to 11 wt. % silicon,
greater than or equal to 0.01 wt. % to less than or equal to 0.6 wt. % manganese, and
greater than or equal to 75 wt. % to less than or equal to 88 wt. % aluminum.

### Claim 7 (depends on 1)

The method of claim 1, wherein the precursor powder comprises:
greater than or equal to 4 wt. % to less than or equal to 8 wt. % copper,
greater than or equal to 8 wt. % to less than or equal to 11 wt. % silicon,
greater than or equal to 0.01 wt. % to less than or equal to 0.6 wt. % magnesium, and
greater than or equal to 75 wt. % to less than or equal to 88 wt. % aluminum.

### Claim 8 (depends on 1)

The method of claim 1, wherein the precursor powder comprises:
greater than or equal to 4 wt. % to less than or equal to 8 wt. % copper,
greater than or equal to 8 wt. % to less than or equal to 11 wt. % silicon,
greater than or equal to 0.01 wt. % to less than or equal to 0.3 wt. % titanium, and
greater than or equal to 75 wt. % to less than or equal to 88 wt. % aluminum.

### Claim 9 (depends on 1)

The method of claim 1, wherein the precursor powder comprises:
greater than or equal to 4 wt. % to less than or equal to 8 wt. % copper,
greater than or equal to 8 wt. % to less than or equal to 11 wt. % silicon,
greater than or equal to 0.01 wt. % to less than or equal to 0.8 wt. % iron,
greater than or equal to 0.01 wt. % to less than or equal to 0.6 wt. % manganese,
greater than or equal to 0.01 wt. % to less than or equal to 0.6 wt. % magnesium,
greater than or equal to 0.01 wt. % to less than or equal to 0.3 wt. % titanium, and
greater than or equal to 75 wt. % to less than or equal to 88 wt. % aluminum.

### Claim 10 (depends on 1)

The method of claim 1, further comprising preparing the precursor powder, wherein preparing the precursor powder comprises combining a copper-containing powder with a silicon-containing powder.

### Claim 11 (depends on 1)

The method of claim 1, further comprising preparing the precursor powder, wherein preparing the precursor powder comprises combining an elemental copper powder with a pre-alloyed powder comprising silicon, aluminum, magnesium, or combinations thereof.

### Claim 12 (depends on 1)

The method of claim 1, further comprising preparing the precursor powder, wherein preparing the precursor powder comprises sizing the precursor powder to an average particle size of greater than or equal to 1 μm to less than or equal to 100 μm.

### Claim 13 (depends on 1)

The method of claim 1, further comprising preparing the precursor powder, wherein preparing the precursor powder comprises sizing the precursor powder to a particle size distribution of 1 μm to 100 μm.

### Claim 14 (depends on 1)

The method of claim 1, further comprising preparing the precursor powder, wherein preparing the precursor powder comprises sizing the precursor powder via vibratory sieving.

### Claim 15 (depends on 1)

The method of claim 1, further comprising preparing the precursor powder, wherein preparing the precursor powder comprises ultrasonic atomization.

### Claim 16 (depends on 1)

The method of claim 1, further comprising (e) repeating steps (c) through (d) a plurality of times.

### Claim 17 (depends on 1)

The method of claim 1, wherein the three-dimensional article has a density of greater than or equal to 99.2%.

### Claim 18 (depends on 1)

The method of claim 1, wherein the three-dimensional article has a density of greater than or equal to 99.5%.

### Claim 19 (depends on 1)

The method of claim 1, wherein the three-dimensional article has a density of greater than or equal to 99.9%.

### Claim 20 (depends on 1)

The method of claim 1, wherein the alloy has a hardness of greater than or equal to 140 HV to 200 HV, a hot crack susceptibility coefficient of less than or equal to 0.3, and a density of 99.2% or greater.

### Claim 21

A method for producing an alloy structure having a density of greater than or equal to 99.2%, comprising:
providing a precursor powder comprising greater than or equal to 4 wt. % to less than or equal to 8 wt. % copper to an additive manufacturing system; and
contacting the precursor powder with an energy source to form the alloy structure.

### Claim 22

An alloy, comprising:
greater than or equal to 4 wt. % to less than or equal to 8 wt. % copper,
greater than or equal to 8 wt. % to less than or equal to 11 wt. % silicon, and
greater than or equal to 75 wt. % to less than or equal to 88 wt. % aluminum,
wherein the alloy has a hardness of greater than or equal to 140 HV to less than or equal to 200 HV, a hot crack susceptibility coefficient of less than or equal to 0.3, and a density of greater than or equal to 99.5%.