# US 2025/0084500 A1 · Low-carbon, low-alloy and high-formability dual-phase steel having tensile strength of greater than or equal to 590 mpa, hot-dip galvanized dual-phase steel, and manufacturing method therefor

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2025/0084500 A1
- Document ID: US20250084500A1
- Status: Published application
- Kind: A1
- Application number: 18/552,929
- Filed: 2022-03-31
- Published: 2025-03-13
- Earliest claimed: 2021-04-02
- Assignees: Baoshan Iron & Steel Co., Ltd.
- Applicants: Baoshan Iron & Steel Co., Ltd.
- Inventors: Jun LI; Jian WANG; Junfei WANG; Chao WANG; Baoping ZHANG; Huafei LIU; Jingge DAI; Yimin LIU; Fengzhi LU; Honglin YANG
- Web page: https://patentgrep.com/patent/US20250084500A1

## CPC

- C21D 9/0081: {for slabs; for billets}
- B32B 15/013: {one layer being formed of an iron alloy or steel, another layer being formed of a metal other than iron or aluminium}
- B32B 15/017: {one layer being formed of aluminium or an aluminium alloy, another layer being formed of an alloy based on a non ferrous metal other than aluminium}
- C21D 1/18: Hardening (C21D1/02 takes precedence); Quenching with or without subsequent tempering (quenching devices C21D1/62)
- C21D 6/002: {containing Cr (C21D6/004 takes precedence)}
- C21D 6/005: {containing Mn}
- C21D 6/008: {containing Si}
- C21D 8/02: during manufacturing of plates or strips (C21D8/12 takes precedence)
- C21D 8/0226: {Hot rolling}
- C21D 8/0236: {Cold rolling}
- C21D 8/0263: {following hot rolling}
- C21D 8/0273: {Final recrystallisation annealing}
- C21D 8/0278: involving a particular surface treatment (C21D8/0294 takes precedence)
- C21D 9/46: for sheet metals
- C22C 38/002: {containing In, Mg, or other elements not provided for in one single group C22C38/001 - C22C38/60}
- C22C 38/02: containing silicon
- C22C 38/04: containing manganese
- C22C 38/06: containing aluminium
- C22C 38/12: containing tungsten, tantalum, molybdenum, vanadium, or niobium
- C22C 38/14: containing titanium or zirconium
- C22C 38/18: containing chromium
- C22C 38/22: with molybdenum or tungsten
- C22C 38/24: with vanadium
- C22C 38/26: with niobium or tantalum
- C22C 38/28: with titanium or zirconium
- C22C 38/38: with more than 1.5% by weight of manganese
- C23C 2/0224: {Two or more thermal pretreatments}
- C23C 2/06: Zinc or cadmium or alloys based thereon
- C23C 2/285: {for remelting the coating}
- C23C 2/29: {Cooling or quenching}
- C23C 2/40: Plates; Strips
- B32B 2311/20: Zinc
- C21D 2211/005: Ferrite
- C21D 2211/008: Martensite
- C21D: MODIFYING THE PHYSICAL STRUCTURE OF FERROUS METALS; GENERAL DEVICES FOR HEAT TREATMENT OF FERROUS OR NON-FERROUS METALS OR ALLOYS; MAKING METAL MALLEABLE, e.g. BY DECARBURISATION OR TEMPERING (surface treatment of metallic material involving at least one process provided for in class C23 and at least one process covered by this subclass C23F17/00; unidirectional solidification of eutectic materials or unidirectional demixing of eutectoid materials C30B)
- B32B: LAYERED PRODUCTS, i.e. PRODUCTS BUILT-UP OF STRATA OF FLAT OR NON-FLAT, e.g. CELLULAR OR HONEYCOMB, FORM
- C22C: ALLOYS (treatment of alloys C21D, C22F)
- C23C: COATING METALLIC MATERIAL; COATING MATERIAL WITH METALLIC MATERIAL; SURFACE TREATMENT OF METALLIC MATERIAL BY DIFFUSION INTO THE SURFACE, BY CHEMICAL CONVERSION OR SUBSTITUTION; COATING BY VACUUM EVAPORATION, BY SPUTTERING, BY ION IMPLANTATION OR BY CHEMICAL VAPOUR DEPOSITION, IN GENERAL (making metal-coated products by extrusion B21C23/22; covering with metal by connecting pre-existing layers to articles, see the relevant places, e.g. B21D39/00, B23K; metallising of glass C03C; metallising mortars, concrete, artificial stone, ceramics or natural stone C04B41/00; enamelling of, or applying a vitreous layer to, metals C23D; treating metal surfaces or coating of metals by electrolysis or electrophoresis C25D; single-crystal film growth C30B; by metallising textiles D06M11/83; decorating textiles by locally metallising D06Q1/04)

## Abstract

A low-carbon, low-alloy and high-formability dual-phase steel having a tensile strength of greater than or equal to 590 MPa, a hot-dip galvanized dual-phase steel, and a manufacturing method therefor by means of rapid heat treatment. The steel comprises the following components, in percentage by mass: 0.04-0.12% of C, 0.1-0.5% of Si, 1.0-2.0% of Mn, P≤0.02%, S≤0.015%, 0.02-0.06% of Al, and can further comprise one or two of Cr, Mo, Ti, Nb and V, wherein Cr+Mo+Ti+Nb+V≤0.5%, and the balance is Fe and other unavoidable impurities. The manufacturing method therefor includes smelting, casting, hot rolling, cold rolling, and rapid heat treatment processes. In the present invention, by controlling rapid heating, short-term thermal insulation and rapid cooling processes during the process of rapid heat treatment, the recovery of a deformed structure, recrystallization and austenite transformation processes are changed, the nucleation rate is increased, the grain growth time is shortened, grains are refined, the strength and n value of the material are improved, and the interval range of the material performance is expanded.

## Claims

### Claim 1

A low carbon low alloy dual-phase steel with high formability or hot-galvanized dual-phase steel with high formability having a tensile strength of ≥590 MPa, which comprises the following chemical components in mass percentages: C: 0.04˜0.12%, Si: 0.1˜0.5%, Mn: 1.0˜2.0%, P≤0.02%, S≤0.015%, Al: 0.02˜0.06%, optionally one or two of Cr, Mo, Ti, Nb, V, and Cr+Mo+Ti+Nb+V≤0.5%, with a balance of Fe and other unavoidable impurities.

### Claim 2 (depends on 1)

The low carbon low alloy dual-phase steel with high formability or hot-galvanized dual-phase steel with high formability having a tensile strength of ≥590 MPa according to claim 1,
wherein the dual-phase steel or hot-galvanized dual-phase steel has a yield strength of 340˜560 MPa, a tensile strength of 620˜880 MPa, an elongation of 19˜30.5%, a product of strength and elongation of 15.5˜20.5 GPa % and a strain hardening index n90 value greater than 0.20; and/or
wherein the microstructure of the dual-phase steel or hot-galvanized dual-phase steel is a dual-phase structure of ferrite and martensite having an average grain size of 2˜10 μm.

### Claim 3 (depends on 1)

The low carbon low alloy dual-phase steel with high formability or hot-galvanized dual-phase steel with high formability having a tensile strength of ≥590 MPa according to claim 1, wherein the low carbon low alloy dual-phase steel with high formability having a tensile strength of ≥590 MPa is obtained by the following process:
1) Smelting, casting
wherein the above components are subjected to smelting and casting to form a slab;
2) hot rolling, coiling
wherein a hot rolling finishing temperature is ≥Ar3; and a coiling temperature is 550˜680° C.;
3) cold rolling
wherein a cold rolling reduction rate is 40˜85%;
4) Rapid heat treatment
wherein the steel plate after cold rolling is rapidly heated to 750˜845° C., wherein the rapid heating is performed in one stage or two stages; when the rapid heating is performed in one stage, a heating rate is 50˜500° C./s; when the rapid heating is performed in two stages, the steel plate is heated in the first stage from room temperature to 550˜650° C. at a heating rate of 15˜500° C./s, heated in the second stage from 550˜650° C. to 750˜845° C. at a heating rate of 30˜500° C./s (such as 50˜500° C./s); then soaked at a soaking temperature of 750˜845° C. for a soaking time of 10˜60 s;
wherein after soaking, the steel plate is slowly cooled to 670˜770° C. at a cooling rate of 5˜15° C./s, then rapidly cooled from 670˜770° C. to room temperature at a cooling rate of 50˜200° C./s;
or the steel plate is rapidly cooled from 670˜770° C. to 230˜280° C. at a cooling rate of 50˜200° C./s, and over-aged in this temperature range, wherein an over-ageing treating time is less than or equal to 200 s; and finally cooled to room temperature at a cooling rate of 30˜50° C./s.

### Claim 4 (depends on 3)

The low carbon low alloy dual-phase steel with high formability or hot-galvanized dual-phase steel with high formability having a tensile strength of ≥590 MPa according to claim 3, wherein the process has one or more of the following features:
in step 4), a total time of the rapid heat treatment is 41˜300 s or 41˜296 s;
in step 2), the coiling temperature is 580˜650° C.;
in step 3), the cold rolling reduction rate is 60˜80%;
in step 4), when the rapid heating is performed in one stage, the heating rate is 50˜300° C./s;
in step 4), the rapid heating is performed in two stages, wherein the steel plate is heated in the first stage from room temperature to 550˜650° C. at a heating rate of 15˜300° C./s, heated in the second stage from 550˜650° C. to 750˜845° C. at a heating rate of 50˜300° C./s; or the steel plate is heated in the first stage from room temperature to 550˜650° C. at a heating rate of 50˜300° C./s, heated in the second stage from 550˜650° C. to 750˜845° C. at a heating rate of 80˜300° C./s;
in step 4), the soaking time is 10˜40 s;
in step 4), the rapid cooling rate of the steel plate is 50˜150° C./s; and
the over ageing time is 20˜200 s.

### Claim 5 (depends on 1)

The low carbon low alloy dual-phase steel with high formability or hot-galvanized dual-phase steel with high formability having a tensile strength of ≥590 MPa according to claim 1, wherein:
(1) the low carbon low alloy dual-phase steel with high formability comprises the following chemical components in mass percentages: C: 0.04˜0.10%, Si: 0.1˜0.3%, Mn: 1.0˜1.6%, P≤0.02%, S≤0.015%, Al: 0.02˜0.06%, optionally one or two of Cr, Mo, Ti, Nb, V, and Cr+Mo+Ti+Nb+V≤0.5%, with a balance of Fe and other unavoidable impurities; or
(2) the low carbon low alloy dual-phase steel with high formability comprises the following chemical components in mass percentages: C: 0.05˜0.12%, Si: 0.01˜0.5%, Mn: 1.2˜2.0%, P≤0.015%, S≤0.003%, Al: 0.02˜0.055%, optionally one or two of Cr, Mo, Ti, Nb, V, and Cr+Mo+Ti+Nb+V≤0.5%, with a balance of Fe and other unavoidable impurities; or
(3) the low carbon low alloy dual-phase steel with high formability comprises the following chemical components in mass percentages: C: 0.045˜0.12%, Si: 0.1˜0.5%, Mn: 1.0˜2.0%, P≤0.02%, S≤0.006%, Al: 0.02˜0.055%, optionally one or two of Cr, Mo, Ti, Nb, V, and Cr+Mo+Ti+Nb+V≤0.5%, with a balance of Fe and other unavoidable impurities.

### Claim at position 6

-7. (canceled)

### Claim 8 (depends on 5)

The low carbon low alloy dual-phase steel with high formability or hot-galvanized dual-phase steel with high formability having a tensile strength of ≥590 MPa according to claim 5, wherein after the end of soaking step and the steel is slowly cooled to 670˜770° C., it is rapidly cooled to 460˜470° C. at a cooling rate of 50˜200° C./s and immersed in a zinc pot for hot galvanizing to obtain the hot-galvanized dual phase steel;
optionally, after hot galvanizing, the steel is rapidly cooled to room temperature at a cooling rate of 30˜150° C./s to obtain a hot dip galvanized GI product or after hot galvanizing, the steel is heated to 480˜550° C. at a heating rate of 30˜200° C./s and alloyed for 10˜20 s;
optionally, after alloying, the steel is rapidly cooled to room temperature at a cooling rate of 30˜250° C./s to obtain an alloy galvannealed GA product.

### Claim 9 (depends on 1)

The low carbon low alloy dual-phase steel with high formability or hot-galvanized dual-phase steel with high formability having a tensile strength of ≥590 MPa according to claim 1, wherein the hot-galvanized dual-phase steel comprises the following chemical components in mass percentages: C: 0.045˜0.105%, Si: 0.1˜0.4%, Mn: 1.0˜1.5%, P≤0.02%, S≤0.006%, Al: 0.02˜0.055%, optionally one or two of Cr, Mo, Ti, Nb, V, and Cr+Mo+Ti+Nb+V≤0.3%, with a balance of Fe and other unavoidable impurities.

### Claim 10 (depends on 1)

The low carbon low alloy dual-phase steel with high formability or hot-galvanized dual-phase steel with high formability having a tensile strength of ≥590 MPa according to claim 1, wherein the hot-galvanized dual-phase steel comprises the following chemical components in mass percentages: C: 0.05˜0.12%, Si: 0.01˜0.5%, Mn: 1.2˜2.0%, P≤0.015%, S≤0.003%, Al: 0.02˜0.055%, optionally one or two of Cr, Mo, Ti, Nb, V, and Cr+Mo+Ti+Nb+V≤0.5%, with a balance of Fe and other unavoidable impurities.

### Claim 11 (depends on 9)

The low carbon low alloy dual-phase steel with high formability or hot-galvanized dual-phase steel with high formability having a tensile strength of ≥590 MPa according to claim 9, wherein the hot-galvanized dual-phase steel with high formability is obtained by the following process:
a) Smelting, casting
wherein the above components are subjected to smelting and casting to form a slab;
b) Hot rolling, coiling
wherein a hot rolling finishing temperature is ≥Ar3; and a coiling temperature is 550˜680° C.;
c) Cold rolling
wherein a cold rolling reduction rate is 40˜85%;
d) Rapid heat treatment, hot-galvanizing
wherein the steel plate after cold rolling is rapidly heated to 750˜845° C.,
wherein the rapid heating is performed in one stage or two stages;
when the rapid heating is performed in one stage, a heating rate is 50˜500° C./s;
when the rapid heating is performed in two stages, the steel plate is heated in the first stage from room temperature to 550˜650° C. at a heating rate of 15˜500° C./s, heated in the second stage from 550˜650° C. to 750˜845° C. at a heating rate of 30˜500° C./s (such as 50˜500° C./s); then soaked at a soaking temperature of 750˜845° C. for a soaking time of 10˜60 s;
wherein after soaking, the steel plate is slowly cooled to 670˜770° C. at a cooling rate of 5˜15° C./s, then rapidly cooled to 460˜470° C. at a cooling rate of 50˜200° C./s, such as 50˜150° C./s, and immersed in a zinc pot for hot galvanizing;
wherein after hot galvanizing, the steel plate is rapidly cooled to room temperature at a cooling rate of 30˜150° C./s to obtain a hot dip galvanized GI product; or
after hot galvanizing, the steel plate is heated to 480˜550° C. at a heating rate of 30˜200° C./s and alloyed for 10˜20 s; after alloying, the steel plate is rapidly cooled to room temperature at a cooling rate of 30˜250° C./s to obtain an alloy galvannealed GA product.

### Claim 12 (depends on 11)

The low carbon low alloy dual-phase steel with high formability or hot-galvanized dual-phase steel with high formability having a tensile strength of ≥590 MPa according to claim 11, wherein the process has one or more of the following features:
a total time of the rapid heat treatment and hot-galvanizing of step d) is 30˜142 s;
in step b), the coiling temperature is 580˜650° C.;
in step c), the cold rolling reduction rate is 60˜80%;
in step d), when the rapid heating is performed in one stage, the heating rate is 50˜300° C./s;
in step d), the rapid heating is performed in two stages, wherein the steel plate is heated in the first stage from room temperature to 550˜650° C. at a heating rate of 15˜300° C./s, heated in the second stage from 550˜650° C. to 750˜845° C. at a heating rate of 50˜300° C./s; or the steel plate is heated in the first stage from room temperature to 550˜650° C. at a heating rate of 30˜300° C./s, heated in the second stage from 550˜650° C. to 750˜845° C. at a heating rate of 80˜300° C./s

### Claim 13 (depends on 1)

A manufacturing process of low carbon low alloy dual-phase steel with high formability having a tensile strength of ≥590 MPa according to claim 1, which comprises the following steps:
1) Smelting, casting
wherein the above components are subjected to smelting and casting to form a slab;
2) hot rolling, coiling
wherein a hot rolling finishing temperature is ≥Ar3; and a coiling temperature is 550˜680° C.;
3) cold rolling
wherein a cold rolling reduction rate is 40˜85%, thereby obtaining a rolled hard strip steel or steel plate;
4) Rapid heat treatment
a) Rapid heating
wherein the strip steel or steel plate after cold rolling is rapidly heated to 750˜845° C., wherein the rapid heating is performed in one stage or two stages; when the rapid heating is performed in one stage, a heating rate is 50˜500° C./s; when the rapid heating is performed in two stages, the steel plate is heated in the first stage from room temperature to 550˜650° C. at a heating rate of 15˜500° C./s, heated in the second stage from 550˜650° C. to 750˜845° C. at a heating rate of 30˜500° C./s (such as 50˜500° C./s);
b) Soaking
wherein the strip steel or steel plate is soaked at a temperature of 750˜845° C., which is the target temperature of the dual phase region of austenite and ferrite, for a soaking time of 10˜60 s;
c) Cooling
wherein after soaking, the strip steel or steel plate is slowly cooled to 670˜770° C. at a cooling rate of 5˜15° C./s, then rapidly cooled from 670˜770° C. to room temperature at a cooling rate of 50˜200° C./s;
or the strip steel or steel plate is rapidly cooled from 670˜770° C. to 230˜280° C. at a cooling rate of 50˜200° C./s for over-ageing treatment, wherein an over-ageing treating time is less than or equal to 200 s; after over-ageing treatment, it is finally cooled to room temperature at a cooling rate of 30˜50° C./s.

### Claim 14 (depends on 1)

The manufacturing process by rapid heat treatment of the low carbon low alloy hot-galvanized dual-phase steel with high formability having a tensile strength of ≥590 MPa according to claim 1, which comprises the following steps:
A) Smelting, casting
wherein the above components are subjected to smelting and casting to form a slab;
B) Hot rolling, coiling
wherein a hot rolling finishing temperature is ≥Ar3; and a coiling temperature is 550˜680° C.;
C) Cold rolling
wherein a cold rolling reduction rate is 40˜85%, thereby obtaining a rolled hard strip steel or steel plate;
D) Rapid heat treatment, hot-galvanizing
a) rapid heating
wherein the strip steel or steel plate after cold rolling is rapidly heated from room temperature to 750˜845° C., which is the target temperature of dual phase region of austenite and ferrite, wherein the rapid heating is performed in one stage or two stages;
when the rapid heating is performed in one stage, a heating rate is 50˜500° C./s;
when the rapid heating is performed in two stages, the strip steel or steel plate is heated in the first stage from room temperature to 550˜650° C. at a heating rate of 15˜500° C./s, heated in the second stage from 550˜650° C. to 750˜845° C. at a heating rate of 30˜500° C./s (such as 50˜500° C./s);
b) Soaking
wherein the strip steel or steel plate is soaked at a temperature of 750˜845° C., which is the target temperature of the dual phase region of austenite and ferrite, for a soaking time of 10˜60 s;
c) Cooling, hot-galvanizing
wherein after soaking, the strip steel or steel plate is slowly cooled to 670˜770° C. at a cooling rate of 5˜15° C./s, then rapidly cooled to 460˜470° C. at a cooling rate of 50˜150° C./s and immersed in a zinc pot for hot galvanizing;
d) after hot galvanizing, the strip steel or steel plate is rapidly cooled to room temperature at a cooling rate of 50˜150° C./s to obtain a hot dip galvanized GI product; or
after hot galvanizing, the strip steel or steel plate is heated to 480˜550° C. at a heating rate of 30˜200° C./s and alloyed for 10˜20 s; after alloying, the strip steel or steel plate is rapidly cooled to room temperature at a cooling rate of 30˜250° C./s to obtain an alloy galvannealed GA product.

### Claim 15 (depends on 13)

The process according to claim 13 comprises one or more of the following features:
a total time of the rapid heat treatment of step 4) is 41˜300 s or 41˜296 s;
in step 2), the coiling temperature is 580˜650° C.;
in step 3), the cold rolling reduction rate is 60˜80%;
in step 4), when the rapid heating is performed in one stage, the heating rate is 50˜300° C./s;
in step 4), the rapid heating is performed in two stages, wherein the strip steel or steel plate is heated in the first stage from room temperature to 550˜650° C. at a heating rate of 15˜300° C./s, heated in the second stage from 550˜650° C. to 750˜845° C. at a heating rate of 50˜300° C./s, or the strip steel or steel plate is heated in the first stage from room temperature to 550˜650° C. at a heating rate of 50˜300° C./s, heated in the second stage from 550˜650° C. to 750˜845° C. at a heating rate of 80˜300° C./s;
in step 4), the final temperature after rapid heating is 770˜830° C. or 790˜830° C.;
in step 4), the rapid cooling rate of the strip steel or steel plate is 50˜150° C./s;
in the soaking process of step 4) after the strip steel or steel plate is heated to the target temperature of dual phase region of austenite and ferrite, the temperature is kept unchanged for soaking;
in the soaking process of step 4), the strip steel or steel plate is slightly heated up or cooled down in the soaking time, wherein the temperature after heating is no more than 845° C. and the temperature after cooling is no less than 750° C.;
the soaking time is 10˜40 s;
the over ageing time is 20˜200 s.

### Claim 16 (depends on 1)

The low carbon low alloy dual-phase steel with high formability or hot-galvanized dual-phase steel with high formability having a tensile strength of ≥590 MPa according to claim 1, wherein in the dual-phase steel with high formability or the hot-galvanized dual-phase steel with high formability:
the content of C is 0.045˜0.105%, 0.04˜0.10%, 0.05˜1.2%, 0.06˜0.08%, 0.065˜0.085% or 0.07˜0.1%; and/or
the content of Si is 0.1˜0.4%, 0.1˜0.3% or 0.15˜0.25%; and/or
the content of Mn is 1.0˜1.6%, 1.0˜1.5%, 1.2˜2.0%, 1.2˜1.4%, 1.2˜1.35% or 1.5˜1.8%; and/or
Cr+Mo+Ti+Nb+V≤0.3%; and/or
the low carbon low alloy dual-phase steel with high formability having a tensile strength of ≥590 MPa comprises the following chemical components in mass percentages: C: 0.04˜0.105%, Si: 0.1˜0.4%, Mn: 1.0˜1.6%, P≤0.02%, S≤0.015%, Al: 0.02˜0.06%, optionally one or two of Cr, Mo, Ti, Nb, V, and Cr+Mo+Ti+Nb+V≤0.5%, with a balance of Fe and other unavoidable impurities.

### Claim 17 (depends on 5)

The low carbon low alloy dual-phase steel with high formability or hot-galvanized dual-phase steel with high formability having a tensile strength of ≥590 MPa according to claim 5, wherein in (1):
the dual-phase steel has a C content of 0.06˜0.08%; and/or
the dual-phase steel has a Si content of 0.15˜0.25%; and/or
the dual-phase steel has a Mn content of 1.2%˜1.4%; and/or
the microstructure of the dual-phase steel is a dual-phase structure of ferrite and martensite having an average grain size of 4˜10 μm; and/or
the dual-phase steel has a yield strength of 350˜410 MPa, a tensile strength of 620˜710 MPa, an elongation of 24.0˜30.5%, a product of strength and elongation of 17˜20.5 GPa % and a strain hardening index n90 value greater than 0.20; or the dual-phase steel has a yield strength of 350˜405 MPa, a tensile strength of 624˜706 MPa, an elongation of 24.4˜30.4%, a product of strength and elongation of 17˜20.1 GPa % and a strain hardening index n90 value greater than 0.20; and/or
in the manufacturing process of the dual-phase steel, a total time of the rapid heat treatment in step 4) is 41˜300 s.

### Claim 18 (depends on 5)

The low carbon low alloy dual-phase steel with high formability or hot-galvanized dual-phase steel with high formability having a tensile strength of ≥590 MPa according to claim 5, wherein in (2):
the dual-phase steel has a tensile strength of ≥780 MPa; and/or
the dual-phase steel has a C content of 0.07˜0.1%; and/or
the dual-phase steel has a Si content of 0.1˜0.4%; and/or
the dual-phase steel has a Mn content of 1.5%˜1.8%; and/or
the microstructure of the dual-phase steel is a dual-phase structure of ferrite and martensite having an average grain size of 2˜8 μm; and/or
the dual-phase steel has a yield strength of 400˜540 MPa, a tensile strength of 780˜880 MPa, an elongation of 19˜24.5%, a product of strength and elongation of 19˜24.5 GPa % and a strain hardening index n90 value greater than 0.20; or the dual-phase steel has a yield strength of 400˜533 MPa, a tensile strength of 781˜878 MPa, an elongation of 19.5˜24.1%, a product of strength and elongation of 16.3˜19.3 GPa % and a strain hardening index n90 value greater than 0.20; and/or
in the manufacturing process of the dual-phase steel, a total time of the rapid heat treatment in step 4) is 41˜296 s.

### Claim 19 (depends on 9)

The low carbon low alloy dual-phase steel with high formability or hot-galvanized dual-phase steel with high formability having a tensile strength of ≥590 MPa according to claim 9, wherein:
in the hot-galvanized dual-phase steel, the C content is 0.065˜0.085%; and/or
in the hot-galvanized dual-phase steel, the Si content is 0.15˜0.25%; and/or
in the hot-galvanized dual-phase steel, the Mn content is 1.2%˜1.35%; and/or
in the hot-galvanized dual-phase steel, Cr+Mo+Ti+Nb+V≤0.2%; and/or
the dual-phase steel has a yield strength of 340˜410 MPa, a tensile strength of 620˜710 MPa, an elongation of 22˜30.5%, a product of strength and elongation of 15.5˜20.0 GPa % and a strain hardening index n90 value greater than 0.21; or the hot-galvanized dual-phase steel has a yield strength of 347˜405 MPa, a tensile strength of 624˜709 MPa, an elongation of 22.2˜30.3%, a product of strength and elongation of 15.7˜19.6 GPa % and a strain hardening index n90 value greater than 0.21.

### Claim 20 (depends on 10)

The low carbon low alloy dual-phase steel with high formability or hot-galvanized dual-phase steel with high formability having a tensile strength of ≥590 MPa according to claim 10, wherein:
the hot-galvanized dual-phase steel has a yield strength of ≥780 MPa; and/or
the hot-galvanized dual-phase steel has a C content of 0.07˜0.1%; and/or
the hot-galvanized dual-phase steel has a Si content of 0.1˜0.4%; and/or
the hot-galvanized dual-phase steel has a Mn content of 1.5%˜1.8%; and/or
the hot-galvanized dual-phase steel has a yield strength of 400˜560 MPa, a tensile strength of 790˜870 MPa, an elongation of 19.0˜25.0%, a product of strength and elongation of 16.0˜20.0 GPa % and a strain hardening index n90 value greater than 0.20; or the hot-galvanized dual-phase steel has a yield strength of 400˜552 MPa, a tensile strength of 798˜862 MPa, an elongation of 19.5˜24.6%, a product of strength and elongation of 16.3˜19.9 GPa % and a strain hardening index n90 value greater than 0.20.

### Claim 21 (depends on 14)

The process according to claim 14, which comprises one or more of the following features:
a total time of the rapid heat treatment and hot-galvanizing of step D) is 30˜142 s;
in step B), the coiling temperature is 580˜650° C.;
in step C), the cold rolling reduction rate is 60˜80%;
in step D), when the rapid heating is performed in one stage, the heating rate is 50˜300° C./s;
in step D), the rapid heating is performed in two stages, wherein the strip steel or steel plate is heated in the first stage from room temperature to 550˜650° C. at a heating rate of 15˜300° C./s, heated in the second stage from 550˜650° C. to 750˜845° C. at a heating rate of 50˜300° C./s, or the strip steel or steel plate is heated in the first stage from room temperature to 550˜650° C. at a heating rate of 50˜300° C./s, heated in the second stage from 550˜650° C. to 750˜845° C. at a heating rate of 80˜300° C./s;
in step D), the final temperature after rapid heating is 770˜830° C. or 790˜830° C.;
in step D), the rapid cooling rate of the strip steel or steel plate is 50˜150° C./s;
in the soaking process of step D), after the strip steel or steel plate is heated to the target temperature of dual phase region of austenite and ferrite, the temperature is kept unchanged for soaking;
in the soaking process of step D), the strip steel or steel plate is slightly heated up or cooled down in the soaking time, wherein the temperature after heating is no more than 845° C. and the temperature after cooling is no less than 750° C.;
the soaking time is 10˜40 s;
the over ageing time is 20˜200 s;
in step D), after alloying, the strip steel or steel plate is rapidly cooled to room temperature at a cooling rate of 30˜200° C./s to obtain an alloy galvannealed GA product.

### Claim 22 (depends on 10)

The low carbon low alloy dual-phase steel with high formability or hot-galvanized dual-phase steel with high formability having a tensile strength of ≥590 MPa according to claim 10, wherein the hot-galvanized dual-phase steel with high formability is obtained by the following process:
a) Smelting, casting
wherein the above components are subjected to smelting and casting to form a slab;
b) Hot rolling, coiling
wherein a hot rolling finishing temperature is ≥Ar3; and a coiling temperature is 550˜680° C.;
c) Cold rolling
wherein a cold rolling reduction rate is 40˜85%;
d) Rapid heat treatment, hot-galvanizing
wherein the steel plate after cold rolling is rapidly heated to 750˜845° C.,
wherein the rapid heating is performed in one stage or two stages;
when the rapid heating is performed in one stage, a heating rate is 50˜500° C./s;
when the rapid heating is performed in two stages, the steel plate is heated in the first stage from room temperature to 550˜650° C. at a heating rate of 15˜500° C./s, heated in the second stage from 550˜650° C. to 750˜845° C. at a heating rate of 30˜500° C./s (such as 50˜500° C./s); then soaked at a soaking temperature of 750˜845° C. for a soaking time of 10˜60 s;
wherein after soaking, the steel plate is slowly cooled to 670˜770° C. at a cooling rate of 5˜15° C./s, then rapidly cooled to 460˜470° C. at a cooling rate of 50˜200° C./s, such as 50˜150° C./s, and immersed in a zinc pot for hot galvanizing;
wherein after hot galvanizing, the steel plate is rapidly cooled to room temperature at a cooling rate of 30˜150° C./s to obtain a hot dip galvanized GI product; or
after hot galvanizing, the steel plate is heated to 480˜550° C. at a heating rate of 30˜200° C./s and alloyed for 10˜20 s; after alloying, the steel plate is rapidly cooled to room temperature at a cooling rate of 30˜250° C./s to obtain an alloy galvannealed GA product.