# US 2025/0083974 A1 · Core-shell gradient ternary precursor and preparation method and application thereof

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2025/0083974 A1
- Document ID: US20250083974A1
- Status: Published application
- Kind: A1
- Application number: 18/284,452
- Filed: 2022-08-18
- Published: 2025-03-13
- Earliest claimed: 2022-05-09
- Assignees: Jingmen Gem Co., Ltd.
- Applicants: Jingmen Gem Co., Ltd.
- Inventors: Kaihua XU; Xianjin YUE; Kun ZHANG; Wenchao HUA; Cong LI; Xing YANG; Hao LV; Wenfang YUAN; Dongming JIA; Xiaofei XUE; Xueqian LI; Liangjiao FAN; Xing XIANG; Xiaoshuai ZHU; Jiamin SHI; Zhengjie GONG; Daodao YIN
- Web page: https://patentgrep.com/patent/US20250083974A1

## CPC

- C08G 83/001: {Macromolecular compounds containing organic and inorganic sequences, e.g. organic polymers grafted onto silica}
- H01M 10/0525: Rocking-chair batteries, i.e. batteries with lithium insertion or intercalation in both electrodes; Lithium-ion batteries
- C01G 53/50: of the type (MnO2)n-, e.g. Li(NixMn1-x)O2 or Li(MyNixMn1-x-y)O2
- C01G 53/82: Compounds containing nickel, with or without oxygen or hydrogen, and containing two or more other elements
- H01M 4/131: Electrodes based on mixed oxides or hydroxides, or on mixtures of oxides or hydroxides, e.g. LiCoOx
- H01M 4/366: {as layered products}
- H01M 4/525: of mixed oxides or hydroxides containing iron, cobalt or nickel for inserting or intercalating light metals, e.g. LiNiO2, LiCoO2 or LiCoOxFy
- C01P 2004/80: Particles consisting of a mixture of two or more inorganic phases
- C01P 2004/84: one phase coated with the other
- C01P 2006/40: Electric properties
- H01M 2004/028: {Positive electrodes}
- Y02E 60/10: Energy storage using batteries
- C08G: MACROMOLECULAR COMPOUNDS OBTAINED OTHERWISE THAN BY REACTIONS ONLY INVOLVING UNSATURATED CARBON-TO-CARBON BONDS
- H01M: PROCESSES OR MEANS, e.g. BATTERIES, FOR THE DIRECT CONVERSION OF CHEMICAL ENERGY INTO ELECTRICAL ENERGY
- C01G: COMPOUNDS CONTAINING METALS NOT COVERED BY SUBCLASSES C01D OR C01F (metal hydrides {monoborane, diborane or addition complexes thereof} C01B6/00; salts of oxyacids of halogens C01B11/00; peroxides, salts or peroxyacids C01B15/00; thiosulfates, dithionites, polythionates C01B17/64; compounds containing selenium, or tellurium C01B19/00; binary compounds of nitrogen with metals C01B21/06; azides C01B21/08; {compounds containing nitrogen, other non-metals and metal C01B21/082}; metal amides C01B21/092; nitrites C01B21/50; {compounds of noble gases C01B23/0005}; phosphides C01B25/08; salts of oxyacids of phosphorus C01B25/16; carbides C01B32/90; compounds containing silicon C01B33/00; compounds containing boron C01B35/00; compounds having molecular sieve properties but not having base-exchange properties C01B37/00; compounds having molecular sieve and base-exchange properties, e.g. crystalline zeolites, C01B39/00; cyanides C01C3/08; salts of cyanamide C01C3/16; thiocyanates C01C3/20)
- C01P: INDEXING SCHEME RELATING TO STRUCTURAL AND PHYSICAL ASPECTS OF SOLID INORGANIC COMPOUNDS
- Y02E: REDUCTION OF GREENHOUSE GAS [GHG] EMISSIONS, RELATED TO ENERGY GENERATION, TRANSMISSION OR DISTRIBUTION

## Abstract

A core-shell gradient ternary precursor and a preparation method and application thereof. The preparation method includes (1) mixing a terephthalic acid solution with alkaline liquor to obtain a terephthalic acid salt solution, adding a nickel source solution for a reaction to obtain a Ni-MOF solution, mixing the Ni-MOF solution with ammonia water, and adjusting a pH value to obtain a base solution; and (2) adding a nickel-cobalt-manganese ternary mixed salt solution, a liquid alkali solution, and an ammonia-water solution simultaneously to the base solution obtained in step (1) for a co-precipitation reaction, and obtaining the core-shell gradient ternary precursor after aging treatment. The Ni-MOF is pre-prepared and used as a core for the co-precipitation reaction, to obtain the core-shell like precursor with a gradient. Carbon in the core of the core-shell gradient ternary precursor reacts with oxygen, thereby reducing a nickel oxidation state on particle surfaces and reducing crack generation.

## Claims

### Claim 1

A method of preparing a core-shell gradient ternary precursor, wherein the method comprises the following steps of:
(1) mixing a terephthalic acid solution with alkaline liquor to obtain a terephthalic acid salt solution, adding a nickel source solution for a reaction to obtain a Ni-MOF solution, mixing the Ni-MOF solution with ammonia water, and adjusting pH value to obtain a base solution; and
(2) adding a nickel-cobalt-manganese ternary mixed salt solution, a liquid alkali solution, and an ammonia-water solution simultaneously to the base solution obtained in step (1) for a co-precipitation reaction, and obtaining the core-shell gradient ternary precursor after aging treatment.

### Claim 2 (depends on 1)

The method of claim 1, wherein:
the terephthalic acid solution in step (1) has a molar concentration of ranging from 1 mol/L to 3 mol/L;
optionally, the alkaline liquor comprises a potassium hydroxide solution;
optionally, the alkaline liquor has a molar concentration of ranging from 2 mol/L to 6 mol/L;
optionally, the terephthalic acid salt solution has a pH value of ranging from 6 to 7;
optionally, the nickel source solution comprises a nickel nitrate solution;
optionally, the nickel nitrate solution has a molar concentration of ranging from 1 mol/L to 3 mol/L; and
optionally, a molar ratio of the terephthalic acid to the nickel element in the nickel source is 1:(0.8-1.2).

### Claim 3 (depends on 1)

The method of claim 1, wherein:
stirring is performed in a process of the reaction in step (1);
optionally, a stirring time is in a range from 24 h to 48 h;
optionally, filtration, washing, and drying are performed after the reaction;
optionally, a washing agent for the washing comprises anhydrous ethanol; and
optionally, the drying is performed at a temperature of ranging from 40° C. to 60° C.

### Claim 4 (depends on 1)

The method of claim 1, wherein:
the ammonia water in the base solution in step (1) has a mass concentration of ranging from 4 g/L to 8 g/L;
optionally, Ni-MOF in the base solution has a mass concentration of ranging from 50 g/L to 150 g/L; and
optionally, the base solution has a pH valve of ranging from 11 to 12.

### Claim 5 (depends on 1)

The method of claim 1, wherein:
a solute in the nickel-cobalt-manganese ternary mixed salt solution in step (2) has a mass concentration of ranging from 80 g/L to 120 g/L;
optionally, the nickel-cobalt-manganese ternary mixed salt solution is added at a rate of ranging from 6 L/h to 10 L/h;
optionally, the liquid alkali solution has a mass concentration of ranging from 28% to 32%;
optionally, the liquid alkali solution is added at a rate of ranging from 2 L/h to 3 L/h;
optionally, the ammonia-water solution has a mass concentration of ranging from 10% to 20%; and
optionally, the ammonia-water solution is added at a rate of ranging from 0.1 L/h to 0.6 L/h.

### Claim 6 (depends on 1)

The method of claim 1, wherein:
the co-precipitation reaction in step (2) is carried out at a stirring rate of ranging from 200 rpm to 400 rpm;
optionally, the co-precipitation reaction is carried out at a pH value of ranging from 10 to 12;
optionally, the co-precipitation reaction is carried out at a temperature of ranging from 40° C. to 60° C.; and
optionally, a particle size is continuously monitored in the process of the co-precipitation reaction, before the particle size meets the requirements, a high-efficiency thickener is used in the process of the reaction to collect all particles and return them to a reaction kettle for continuous reaction and growth, when the particle size D50 reaches a range from 3 μm to 4 μm, feeding is stopped, and the reaction is continued until materials react completely.

### Claim 7 (depends on 1)

A core-shell gradient ternary precursor, wherein the core-shell gradient ternary precursor is prepared by the method of claim 1.

### Claim 8 (depends on 7)

A core-shell gradient ternary positive electrode material, wherein the core-shell gradient ternary positive electrode material is prepared from the core-shell gradient ternary precursor of claim 7.

### Claim 9 (depends on 8)

A positive electrode plate, comprising the core-shell gradient ternary positive electrode material of claim 8.

### Claim 10 (depends on 9)

A lithium-ion battery, comprising the positive electrode plate of claim 9.

### Claim 11 (depends on 2)

The method of claim 2, wherein:
stirring is performed in a process of the reaction in step (1);
optionally, a stirring time is in a range from 24 h to 48 h;
optionally, filtration, washing, and drying are performed after the reaction;
optionally, a washing agent for the washing comprises anhydrous ethanol; and
optionally, the drying is performed at a temperature of ranging from 40° C. to 60° C.

### Claim 12 (depends on 2)

The method of claim 2, wherein:
the ammonia water in the base solution in step (1) has a mass concentration of ranging from 4 g/L to 8 g/L;
optionally, Ni-MOF in the base solution has a mass concentration of ranging from 50 g/L to 150 g/L; and
optionally, the base solution has a pH valve of ranging from 11 to 12.

### Claim 13 (depends on 3)

The method of claim 3, wherein:
the ammonia water in the base solution in step (1) has a mass concentration of ranging from 4 g/L to 8 g/L;
optionally, Ni-MOF in the base solution has a mass concentration of ranging from 50 g/L to 150 g/L; and
optionally, the base solution has a pH valve of ranging from 11 to 12.

### Claim 14 (depends on 2)

The method of claim 2, wherein:
a solute in the nickel-cobalt-manganese ternary mixed salt solution in step (2) has a mass concentration of ranging from 80 g/L to 120 g/L;
optionally, the nickel-cobalt-manganese ternary mixed salt solution is added at a rate of ranging from 6 L/h to 10 L/h;
optionally, the liquid alkali solution has a mass concentration of ranging from 28% to 32%;
optionally, the liquid alkali solution is added at a rate of ranging from 2 L/h to 3 L/h;
optionally, the ammonia-water solution has a mass concentration of ranging from 10% to 20%; and
optionally, the ammonia-water solution is added at a rate of ranging from 0.1 L/h to 0.6 L/h.

### Claim 15 (depends on 3)

The method of claim 3, wherein:
a solute in the nickel-cobalt-manganese ternary mixed salt solution in step (2) has a mass concentration of ranging from 80 g/L to 120 g/L;
optionally, the nickel-cobalt-manganese ternary mixed salt solution is added at a rate of ranging from 6 L/h to 10 L/h;
optionally, the liquid alkali solution has a mass concentration of ranging from 28% to 32%;
optionally, the liquid alkali solution is added at a rate of ranging from 2 L/h to 3 L/h;
optionally, the ammonia-water solution has a mass concentration of ranging from 10% to 20%; and
optionally, the ammonia-water solution is added at a rate of ranging from 0.1 L/h to 0.6 L/h.

### Claim 16 (depends on 4)

The method of claim 4, wherein a:
solute in the nickel-cobalt-manganese ternary mixed salt solution in step (2) has a mass concentration of ranging from 80 g/L to 120 g/L;
optionally, the nickel-cobalt-manganese ternary mixed salt solution is added at a rate of ranging from 6 L/h to 10 L/h;
optionally, the liquid alkali solution has a mass concentration of ranging from 28% to 32%;
optionally, the liquid alkali solution is added at a rate of ranging from 2 L/h to 3 L/h;
optionally, the ammonia-water solution has a mass concentration of ranging from 10% to 20%; and
optionally, the ammonia-water solution is added at a rate of ranging from 0.1 L/h to 0.6 L/h.

### Claim 17 (depends on 2)

The method of claim 2, wherein:
the co-precipitation reaction in step (2) is carried out at a stirring rate of ranging from 200 rpm to 400 rpm;
optionally, the co-precipitation reaction is carried out at a pH value of ranging from 10 to 12;
optionally, the co-precipitation reaction is carried out at a temperature of ranging from 40° C. to 60° C.; and
optionally, a particle size is continuously monitored in the process of the co-precipitation reaction, before the particle size meets the requirements, a high-efficiency thickener is used in the process of the reaction to collect all particles and return them to a reaction kettle for continuous reaction and growth, when the particle size D50 reaches a range from 3 μm to 4 μm, feeding is stopped, and the reaction is continued until materials react completely.

### Claim 18 (depends on 3)

The method of claim 3, wherein:
the co-precipitation reaction in step (2) is carried out at a stirring rate of ranging from 200 rpm to 400 rpm;
optionally, the co-precipitation reaction is carried out at a pH value of ranging from 10 to 12;
optionally, the co-precipitation reaction is carried out at a temperature of ranging from 40° C. to 60° C.; and
optionally, a particle size is continuously monitored in the process of the co-precipitation reaction, before the particle size meets the requirements, a high-efficiency thickener is used in the process of the reaction to collect all particles and return them to a reaction kettle for continuous reaction and growth, when the particle size D50 reaches a range from 3 μm to 4 μm, feeding is stopped, and the reaction is continued until materials react completely.

### Claim 19 (depends on 4)

The method of claim 4, wherein:
the co-precipitation reaction in step (2) is carried out at a stirring rate of ranging from 200 rpm to 400 rpm;
optionally, the co-precipitation reaction is carried out at a pH value of ranging from 10 to 12;
optionally, the co-precipitation reaction is carried out at a temperature of ranging from 40° C. to 60° C.; and
optionally, a particle size is continuously monitored in the process of the co-precipitation reaction, before the particle size meets the requirements, a high-efficiency thickener is used in the process of the reaction to collect all particles and return them to a reaction kettle for continuous reaction and growth, when the particle size D50 reaches a range from 3 μm to 4 μm, feeding is stopped, and the reaction is continued until materials react completely.

### Claim 20 (depends on 5)

The method of claim 5, wherein:
the co-precipitation reaction in step (2) is carried out at a stirring rate of ranging from 200 rpm to 400 rpm;
optionally, the co-precipitation reaction is carried out at a pH value of ranging from 10 to 12;
optionally, the co-precipitation reaction is carried out at a temperature of ranging from 40° C. to 60° C.; and
optionally, a particle size is continuously monitored in the process of the co-precipitation reaction, before the particle size meets the requirements, a high-efficiency thickener is used in the process of the reaction to collect all particles and return them to a reaction kettle for continuous reaction and growth, when the particle size D50 reaches a range from 3 μm to 4 μm, feeding is stopped, and the reaction is continued until materials react completely.