# US 2025/0083401 A1 · Mold for Manufacturing a Thermoset Optical Article, Method for Manufacturing the Mold and Method for Manufacturing the Thermoset Optical Article

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2025/0083401 A1
- Document ID: US20250083401A1
- Status: Published application
- Kind: A1
- Application number: 18/580,650
- Filed: 2022-07-18
- Published: 2025-03-13
- Earliest claimed: 2021-07-19
- Assignees: Essilor International
- Applicants: Essilor International
- Inventors: Nisachon KONGTARA; Laurie MARION; Tipparat LERTWATTANASERI; Pierre FROMENTIN
- Web page: https://patentgrep.com/patent/US20250083401A1

## CPC

- B29D 11/0048: {Moulds for lenses (moulds for plastic articles in general B29C33/00)}
- B29C 33/58: Applying the releasing agents
- B29C 33/60: Releasing, lubricating or separating agents {(in general C10M)}
- B29C 33/72: Cleaning {(extruder parts B29C48/27; in general B08B7/00)}
- B29D 11/00125: {Auxiliary operations, e.g. removing oxygen from the mould, conveying moulds from a storage to the production line in an inert atmosphere}
- B29D 11/00865: {Applying coatings; tinting; colouring (printing, marking or copying processes B41M; identification in general G09F3/00; producing decorative effects in general B44C; positioning or marking of lenses B24B13/0055)}
- B29D 11/00326: {having particular surface properties, e.g. a micropattern}
- B29K 2075/00: Use of {PU, i.e.} polyureas or polyurethanes {or derivatives thereof}, as moulding material
- B29K 2909/08: Glass
- B29K 2995/0031: Refractive
- B29L 2011/0016: {Lenses}
- B29D: PRODUCING PARTICULAR ARTICLES FROM PLASTICS OR FROM SUBSTANCES IN A PLASTIC STATE (making granules B29B9/00; making preforms B29B11/00)
- B29C: SHAPING OR JOINING OF PLASTICS; SHAPING OF MATERIAL IN A PLASTIC STATE, NOT OTHERWISE PROVIDED FOR; AFTER-TREATMENT OF THE SHAPED PRODUCTS, e.g. REPAIRING (making preforms B29B11/00; making laminated products by combining previously unconnected layers which become one product whose layers will remain together B32B37/00 - B32B41/00)
- B29K: INDEXING SCHEME ASSOCIATED WITH SUBCLASSES B29B, B29C OR B29D, RELATING TO MOULDING MATERIALS OR TO MATERIALS FOR {MOULDS, } REINFORCEMENTS, FILLERS OR PREFORMED PARTS, e.g. INSERTS
- B29L: INDEXING SCHEME ASSOCIATED WITH SUBCLASS B29C, RELATING TO PARTICULAR ARTICLES

## Abstract

A mold for manufacturing a thermoset optical article having a high refractive index, a method for manufacturing the mold, and a method for manufacturing the article. The mold (1) is configured for manufacturing a thermoset optical article capable of being a poly thiourethane-based lens substrate having a refractive index of from 1.54 to 1.74, by casting a thermosetting material (6) into a molding cavity (5) of the mold, the mold comprising a mineral first mold part (2) having a mineral first inner surface (2a) modified by an organosilane mold-release agent. The modified first inner surface (4) comprises a product of a dehydration-condensation reaction of a hydrolysate of an aqueous alcohol solution of the organosilane mold-release agent applied to the mineral first inner surface (2a) and cured thereon, and the modified first inner surface (4) is devoid of a coating layer of particles and is configured to be directly in contact with the cast thermosetting material.

## Claims

### Claim 1

A mold configured for manufacturing a thermoset optical article capable of being a polythiourethane-based lens substrate having a refractive index of from 1.54 to 1.74, by casting a thermosetting material into a molding cavity of the mold, the mold comprising a mineral first mold part having a mineral first inner surface modified by an organosilane mold-release agent,
wherein the modified first inner surface comprises a product of a dehydration-condensation reaction of a hydrolysate of an aqueous alcohol solution of the organosilane mold-release agent applied to the mineral first inner surface and cured thereon, and
wherein the modified first inner surface is devoid of a coating layer of particles and is configured to be directly in contact with the cast thermosetting material.

### Claim 2 (depends on 1)

The mold according to claim 1, wherein said aqueous alcohol solution comprises a mixture of polar protic solvents comprising water, an alcohol, and a carboxylic acid, said aqueous alcohol solution being optionally devoid of an aprotic solvent.

### Claim 3 (depends on 1)

The mold according to claim 1, wherein said product of the dehydration-condensation reaction results from a curing of said hydrolysate in an oven at a temperature of between 90 and 130° C.

### Claim 4 (depends on 1)

The mold according to claim 1, wherein the organosilane mold-release agent is an aliphatic organoalkoxysilane.

### Claim 5 (depends on 1)

The mold according to claim 1, wherein said aqueous alcohol solution, in which a volume/volume concentration of the organosilane mold-release agent is equal to or greater than 0.05%, is applied to said mineral first inner surface by dipping the mineral first mold part in said aqueous alcohol solution.

### Claim 6 (depends on 1)

The mold according to claim 1, wherein said modified first inner surface is provided, via covalent bonds, with reactive silanol groups formed from said product of the dehydration-condensation reaction, said reactive silanol groups rendering said modified first inner surface hydrophobic even after a plurality of acid washing cycles implemented by immersion during 170 to 190 seconds at 85-95° C. of the modified first inner surface in a bath of sulfuric acid concentrated at at least 98% in weight.

### Claim 7 (depends on 1)

The mold according to claim 1, wherein the mold is further configured to impart to the manufactured thermoset optical article a microstructured main surface, said modified first inner surface having a microstructured pattern configured to directly form said microstructured main surface after casting the thermosetting material in contact with the microstructured pattern.

### Claim 8 (depends on 1)

The mold according to claim 1, wherein the mold further comprises a mineral second mold part which has a mineral second inner surface opposite to the mineral first inner surface, the molding cavity being defined between the modified first inner surface and the mineral second inner surface, which is modified identically to the modified first inner surface by comprising said product of the dehydration-condensation reaction.

### Claim 9 (depends on 1)

A method for manufacturing a mold according to claim 1, wherein the method comprises:
a) Preparing said hydrolysate of the aqueous alcohol solution of the organosilane mold-release agent;
b) Applying the hydrolysate to said mineral first inner surface; and
c) Carrying out said dehydration-condensation reaction of the hydrolysate by curing the applied hydrolysate on the mineral first inner surface, to obtain said modified first inner surface without covering it by a coating layer of particles.

### Claim 10 (depends on 9)

The method for manufacturing a mold according to claim 9, wherein:
step a) successively comprises:
a1) stirring a mixture of several polar protic solvents;
a2) dropwise adding the organosilane mold-release agent to the stirred mixture to obtain a hydrolysable solution; and
a3) hydrolyzing the hydrolysable solution to obtain said hydrolysate;
and/or
step b) successively comprises:
b1) dipping the mineral first mold part in said aqueous alcohol solution; and
b2) drying the dipped mineral first mold part at a temperature of between 20 and 30° C.;
and/or
step c) successively comprises:
c1) implementing said curing in an oven during 10 to 20 minutes at a temperature of 90 to 130° C.; and
c2) cooling down the cured applied hydrolysate at a temperature of between 20 and 30° C.

### Claim 11 (depends on 10)

The method for manufacturing a mold according to claim 10, wherein in step c) said modified first inner surface is provided, via covalent bonds, with reactive silanol groups rendering said modified first inner surface hydrophobic, and wherein the method further comprises, either between sub-steps b1) and b2) or after sub-step c2), an additional washing sub-step by ethanol followed by a drying sub-step at a temperature of between 20 and 30° C., to remove some unreacted silanols from said modified first inner surface.

### Claim 12 (depends on 9)

The method for manufacturing a mold according to claim 9, wherein said mineral first inner surface onto which said hydrolysate is applied in step b) has a microstructured pattern configured to directly form said microstructured main surface after casting the thermosetting material in contact with the microstructured pattern.

### Claim 13 (depends on 1)

A method for manufacturing a thermoset optical article, by casting a thermosetting material into a molding cavity of a mold according to claim 1, wherein the method comprises:
A) at least one washing and/or cleaning cycle;
B) casting the thermosetting material into the molding cavity, so that the thermosetting material directly contacts said modified first inner surface, which is devoid of said coating layer of particles, and an opposite second inner surface of a mineral second mold part of the mold which is modified identically to the modified first inner surface by comprising said product of the dehydration-condensation reaction;
C) curing the thermosetting material cast in the molding cavity; and
D) demolding the molded thermoset material obtained in step C), comprising releasing the molded thermoset material from the modified first inner surface and second inner surface.

### Claim 14 (depends on 13)

The method for manufacturing a thermoset optical article according to claim 13, wherein in step A), said at least one washing and/or cleaning cycle successively comprises:
an acid washing, implemented by immersing during a plurality of minutes at 85-95° C. said modified first inner surface and second inner surface of the mold in a bath of concentrated sulfuric acid;
a dry cleaning of the acid-washed modified first inner surface and second inner surface of the mold, by wiping them with a dry cloth; and
a final aqueous washing of the acid-washed and cleaned modified first inner surface and second inner surface, by dipping into an aqueous alcohol bath comprising ethanol and deionized water.

### Claim 15 (depends on 13)

The method for manufacturing a thermoset optical article according to claim 13, wherein both the thermosetting material cast in step B) and the demolded thermoset material obtained in step D) are free of any mold-release agent, and wherein the demolded thermoset material is devoid of an external layer of embedded particles.

### Claim 16 (depends on 2)

The mold according to claim 2, wherein said aqueous alcohol solution comprises said mixture of polar protic solvents comprising water, said alcohol which is ethanol, methanol or isopropanol, and said carboxylic acid which is acetic acid, said aqueous alcohol solution being devoid of said aprotic solvent which is a fluorous solvent.

### Claim 17 (depends on 3)

The mold according to claim 3, wherein said product of the dehydration-condensation reaction results from the curing of said hydrolysate in the oven at a temperature of between 100 and 120° C. during more than 10 minutes.

### Claim 18 (depends on 4)

The mold according to claim 4, wherein said aliphatic organoalkoxysilane is selected from dimethyl dimethoxysilane (DMDMS), decyltrimethoxysilane (DTMS), triethoxyoctylsilane (OTES) and tridecafluorooctyltriethoxysilane (TDFOTES).

### Claim 19 (depends on 10)

The method for manufacturing a mold according to claim 10, wherein:
step a) successively comprises:
a1) stirring the mixture of several polar protic solvents comprising water, an alcohol which is ethanol, methanol or isopropanol, and a carboxylic acid which is acetic acid;
a2) dropwise adding the organosilane mold-release agent to the stirred mixture to obtain a hydrolysable solution, at a volume/volume concentration of the organosilane mold-release agent in the hydrolysable solution of between 0.05 and 1.5%; and
a3) hydrolyzing the hydrolysable solution to obtain said hydrolysate during 10 to 20 minutes;
step b1) comprises dipping the mineral first mold part in said aqueous alcohol solution during at least 8 minutes; and
step c1) comprises implementing said curing in an oven during 10 to 20 minutes at a temperature of between 100 and 120° C.

### Claim 20 (depends on 13)

The method according to claim 13 for manufacturing a thermoset optical article, which is a polythiourethane-based lens substrate having a refractive index of from 1.54 to 1.74, wherein in step A), the least one washing and/or cleaning cycle comprises an immersion of said modified first inner surface of the mold in an acid bath.