# US 2024/0410044 A1 · Modified Tin-Phosphor Bronze Alloy and A Preparation Method Thereof

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2024/0410044 A1
- Document ID: US20240410044A1
- Status: Published application
- Kind: A1
- Application number: 18/666,687
- Filed: 2024-05-16
- Published: 2024-12-12
- Earliest claimed: 2023-06-08
- Assignees: Chinalco Research Institute of Science and Technology Co., Ltd; China Copper Industry Co., Ltd
- Applicants: Chinalco Research Institute of Science and Technology Co., Ltd; China Copper Industry Co., Ltd
- Inventors: Zhongping CHEN; Huafen LOU; Chaojian XIANG; Hu WANG; Yongda MO; Miaomiao WANG
- Web page: https://patentgrep.com/patent/US20240410044A1

## CPC

- C22F 1/08: of copper or alloys based thereon
- B22D 11/004: {Copper alloys}
- B22D 11/045: for horizontal casting (B22D11/049 - B22D11/059 take precedence)
- C22C 9/02: with tin as the next major constituent
- C22F 1/02: in inert or controlled atmosphere or vacuum (adjusting the composition of the atmosphere C21D1/76)
- C22F 1/06: of magnesium or alloys based thereon
- C22F: CHANGING THE PHYSICAL STRUCTURE OF NON-FERROUS METALS AND NON-FERROUS ALLOYS (surface treatment of metallic material involving at least one process provided for in class C23 and at least one process covered by this subclass, C23F17/00)
- B22D: CASTING OF METALS; CASTING OF OTHER SUBSTANCES BY THE SAME PROCESSES OR DEVICES (shaping of plastics or substances in a plastic state B29C; metallurgical processing, selection of substances to be added to metal C21, C22)
- C22C: ALLOYS (treatment of alloys C21D, C22F)

## Abstract

The disclosure provides a modified tin-phosphor bronze alloy and a preparation method thereof. The modified tin-phosphor bronze alloy comprises the following elements in percentage by mass: 4.0-10 wt % of Sn, 0.01-0.3 wt % of P and the balance of Cu and inevitable impurity elements, the average grain size of the modified tin-phosphor bronze alloy is 1-3 μm, the grain size is in normal distribution, and the standard deviation of the grain size is below 0.8 μm; the proportion of the total low-CSL grain boundary in the modified tin-phosphor bronze alloy in the whole grain boundary is 66-74%, and in the total low-ΣCSL grain boundary, the ratio range of (Σ9+Σ27)/Σ3 is (0.12-0.23):1. The modified tin-phosphor bronze alloy of this disclosure enables a finished alloy can give consideration to both tensile strength and excellent bending performance.

## Claims

### Claim 1

A modified tin-phosphor bronze alloy comprising the following elements in percentage by mass: 4.0-10 wt % of Sn, 0.01-0.3 wt % of P and the balance of Cu and inevitable impurity elements, wherein, the average grain size of the modified tin-phosphor bronze alloy is 1-3 μm, the grain size is in normal distribution, and the standard deviation of the grain size is below 0.8 μm; the proportion of the total low-ΣCSL grain boundary in the modified tin-phosphor bronze alloy in the whole grain boundary is 66-74%, and in the total low-ΣCSL grain boundary, the ratio range of (Σ9+Σ27)/Σ3 is 0.12-0.23:1.

### Claim 2 (depends on 1)

The modified tin-phosphor bronze alloy according to claim 1, wherein, in the total low-ΣCSL grain boundary, the length fraction of the Σ3 grain boundary is 56-61%, the length fraction of the Σ9 grain boundary is 5-8%, and the length fraction of the Σ27 grain boundary is 2.5-4.5%.

### Claim 3 (depends on 1)

The modified tin-phosphor bronze alloy according to claim 1, wherein, the standard deviation is 0.6-0.8 μm.

### Claim 4 (depends on 1)

A preparation method of the modified tin-phosphor bronze alloy according to claim 1, wherein, the preparation method comprises:
subjecting the pretreated tin-phosphor bronze alloy workpiece to modification treatment so as to obtain the modified tin-phosphor bronze alloy;
wherein, the modification treatment comprises a cold rolling deformation step and a heat treatment step carried out sequentially;
wherein, the average grain size of the pretreated tin-phosphor bronze alloy workpiece is 1-3 μm.

### Claim 5 (depends on 4)

The preparation method according to claim 4, wherein, the deformation amount of the cold rolling deformation step is 7-15%.

### Claim 6 (depends on 4)

The preparation method according to claim 4, wherein, the temperature of the heat treatment step is 380-500° C.

### Claim 7 (depends on 5)

The preparation method according to claim 5, wherein, the preparation method further comprises: repeating the modification treatment multiple times.

### Claim 8 (depends on 4)

The preparation method according to claim 4, wherein, the preparation method further comprises a preparation process flow of the pretreated tin-phosphor bronze alloy workpiece, which comprises a batching step, a horizontal continuous casting step, a homogenization annealing step, a face milling step, a cold rolling cogging step, a first recrystallization annealing step, an intermediate rolling deformation step, a second recrystallization annealing step, a finish rolling deformation step, a third recrystallization annealing step, a bottom reservation rolling step, and a fourth recrystallization annealing step carried out sequentially, wherein the temperature of the homogenization annealing step is 650-690° C.

### Claim 9 (depends on 8)

The preparation method according to claim 8, wherein, the temperature of the first recrystallization annealing step is 540-580° C., and the heat preservation time of the first recrystallization annealing step is preferably 4-6 hours.

### Claim 10 (depends on 9)

The preparation method according to claim 9, wherein, the temperature of the third recrystallization annealing step is 650-750° C., and the heat preservation time of the third recrystallization annealing step is preferably 20-60 seconds.

### Claim 11 (depends on 9)

The preparation method according to claim 9, wherein, the atmospheres for the first recrystallization annealing step and the second recrystallization annealing step are each independently a first mixed gas of nitrogen and hydrogen, and the first mixed gas preferably comprises 15-30% of H2 and 70-85% of N2 in percentage by volume; preferably, the atmospheres for the third recrystallization annealing step and the fourth recrystallization annealing step are each independently a second mixed gas of nitrogen and hydrogen, and the second mixed gas preferably comprises 3-5% of H2 and 95-97% of N2 in percentage by volume.

### Claim 12 (depends on 4)

The preparation method according to claim 4, wherein, the heat preservation time of the heat treatment step is 1-4 hours.

### Claim 13 (depends on 7)

The preparation method according to claim 7, wherein, performing 2-5 times of the modification treatment.

### Claim 14 (depends on 8)

The preparation method according to claim 8, wherein, the heat preservation time of the homogenization annealing step is 6-8 hours.

### Claim 15 (depends on 8)

The preparation method according to claim 8, wherein, the deformation amount of the cold rolling cogging step is 80-90%.

### Claim 16 (depends on 8)

The preparation method according to claim 8, wherein, the deformation amount of the bottom reservation rolling step is 40-55%.

### Claim 17 (depends on 8)

The preparation method according to claim 8, wherein, the deformation amount of the intermediate rolling deformation step is preferably 50-70%.

### Claim 18 (depends on 8)

The preparation method according to claim 8, wherein, the deformation amount of the finish rolling deformation step is preferably 40-60%.

### Claim 19 (depends on 8)

The preparation method according to claim 8, wherein, the temperature of the second recrystallization annealing step is 450-500° C., and the heat preservation time of the second recrystallization annealing step is preferably 4-6 hours.

### Claim 20 (depends on 9)

The preparation method according to claim 9, wherein, the temperature of the fourth recrystallization annealing step is 600-650° C., and the heat preservation time of the fourth recrystallization annealing step is preferably 20-60 seconds.