# US 2024/0352624 A1 · Apparatus and method for synthesizing and continuously growing phosphide in magnetic field in immersion fashion

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2024/0352624 A1
- Document ID: US20240352624A1
- Status: Published application
- Kind: A1
- Application number: 18/577,074
- Filed: 2021-12-08
- Published: 2024-10-24
- Earliest claimed: 2021-07-06
- Assignees: The 13th Research Institute of China Electronics Technology Group Corporation
- Applicants: The 13Th Research Institute of China Electronics Technology Group Corporation
- Inventors: Niefeng SUN; Shujie WANG; Senfeng XU; Yanlei SHI; Huimin SHAO; Lijie FU; Aimin BU; Xiaolan LI; Yang WANG
- Web page: https://patentgrep.com/patent/US20240352624A1

## CPC

- C30B 29/44: Gallium phosphide
- C30B 11/003: {Heating or cooling of the melt or the crystallised material}
- C30B 11/04: adding crystallising materials or reactants forming it in situ to the melt
- C30B 15/02: adding crystallising materials or reactants forming it in situ to the melt
- C30B 15/14: Heating of the melt or the crystallised materials
- C30B 15/305: {Stirring of the melt}
- C30B 27/00: Single-crystal growth under a protective fluid
- C30B 27/02: by pulling from a melt
- C30B 29/40: AIIIBV compounds {wherein A is B, Al, Ga, In or Tl and B is N, P, As, Sb or Bi}
- C30B 30/04: using magnetic fields
- Y02P 70/50: Manufacturing or production processes characterised by the final manufactured product
- C30B: SINGLE-CRYSTAL GROWTH (by using ultra-high pressure, e.g. for the formation of diamonds, B01J3/06); UNIDIRECTIONAL SOLIDIFICATION OF EUTECTIC MATERIAL OR UNIDIRECTIONAL DEMIXING OF EUTECTOID MATERIAL; REFINING BY ZONE-MELTING OF MATERIAL (zone-refining of metals or alloys C22B); PRODUCTION OF A HOMOGENEOUS POLYCRYSTALLINE MATERIAL WITH DEFINED STRUCTURE (casting of metals, casting of other substances by the same processes or devices B22D; working of plastics B29; modifying the physical structure of metals or alloys C21D, C22F); SINGLE CRYSTALS OR HOMOGENEOUS POLYCRYSTALLINE MATERIAL WITH DEFINED STRUCTURE; AFTER-TREATMENT OF SINGLE CRYSTALS OR A HOMOGENEOUS POLYCRYSTALLINE MATERIAL WITH DEFINED STRUCTURE (for producing semiconductor devices or parts thereof H10); APPARATUS THEREFOR
- Y02P: CLIMATE CHANGE MITIGATION TECHNOLOGIES IN THE PRODUCTION OR PROCESSING OF GOODS

## Abstract

Device and method for immersed synthesis and continuous growth of phosphides under a magnetic field are disclosed in the field of semiconductor material preparation. In particular, device and method for synthesizing and growing semiconductor phosphides by means of immersing phosphorus into a metal melt under the action of a static magnetic field are disclosed. The device includes a furnace body, an injection synthesis system and a static magnetic field generator. The method includes A, heating the crucible to melt the metal and a covering material boron oxide in the crucible; B, immersing red phosphorus into the crucible; C, applying a static magnetic field surrounding the crucible, and adjusting the temperature gradient to start the synthesis; and D, performing crystal growth after completion of the synthesis. With the method provided by the present invention, the red phosphorus sinks into the melt in the form of a solid and floats upward from the bottom of the crucible after gasification, solving problems such as sucking-back generated by use of phosphorus bubbles; the transverse static magnetic field suppresses the bubble up-floating rate while suppressing the melt convection in the direction of the temperature gradient, so that the synthesis process is smoother and more rapid.

## Claims

### Claim 1

A device for immersed synthesis and growth of phosphides under a magnetic field, comprising a main furnace body, a crucible in the main furnace body, and heaters and thermal insulation layers surrounding the crucible, wherein the device for synthesis and growth further comprises an injection synthesis system connected to a driving device, the injection synthesis system carrying red phosphorus, and immersed into the crucible under an action of the driving device; wherein a static magnetic field generator is disposed outside the main furnace body;
wherein the injection synthesis system comprises a cylindrical red phosphorus injector, and injection holes are formed at the periphery of the red phosphorus injector;
wherein the injection synthesis system also comprises 3-5 disc-shaped shielding layers above the red phosphorus injector, a diameter of the shielding layers is 1 to 10 mm smaller than an inner diameter of the crucible, and the shielding layers are provided with through holes;
wherein, according to positions of the shielding layers, the crucible is divided into different temperature areas, having temperature area ranges between every two shielding layers, above the shielding layer at the top, and below the shielding layer at the bottom; and each temperature area is provided with an independent heater and a thermocouple;
wherein the red phosphorus injector and the shielding layers are connected to the driving device to ascend and descend simultaneously;
wherein, in the thermal insulation layers surrounding the crucible, thermal insulation boards are disposed corresponding to the positions of the shielding layers; and
wherein each of the shielding layers is provided with a thermometer hole at the same position to cooperate with a top thermocouple.

### Claim 2 (depends on 1)

The device of claim 1 for immersed synthesis and growth of phosphides under a magnetic field, wherein the synthesis system is provided with three shielding layers, which are a first shielding layer, a second shielding layer, and a third shielding layer, respectively; the three shielding layers divide the crucible into four temperature areas: a first temperature area above the first shielding layer, a second temperature area between the first shielding layer and the second shielding layer, a third temperature area between the second shielding layer and the third shielding layer, and a fourth temperature area below the third shielding layer; and
wherein the heaters corresponding to respective temperature areas are a first heater, a second heater, a third heater, and a fourth heater, respectively.

### Claim 3 (depends on 1)

A method for immersed synthesis and growth of phosphides under a magnetic field, using the device for immersed synthesis and growth of phosphides under a magnetic field according to claim 1, wherein the method comprises the following steps:
A, heating the crucible to melt the metal and a covering material boron oxide in the crucible;
B, immersing red phosphorus into the crucible;
C, applying a static magnetic field surrounding the crucible, and adjusting the temperature gradient to start the synthesis; and
D, performing crystal growth after completion of the synthesis.

### Claim 4 (depends on 3)

The method according to claim 3,
wherein in step A, the main furnace body is first evacuated to 10−5 Pa to 10 Pa, and then is inflated with an inert gas to be above the saturated vapor pressure at which the melt is heated to the highest pressure; and
wherein the first heater, the second heater, the third heater, and the fourth heater are started to heat at a temperature of 250 to 300° C., and metal in the crucible is formed into a melt.

### Claim 5 (depends on 4)

The method according to claim 4,
wherein in step B, red phosphorus is placed in the red phosphorus injector; and wherein, under the action of the driving device, a low end of the red phosphorus injector is about 5 mm to the bottom of the crucible.

### Claim 6 (depends on 4)

The method according to claim 4,
wherein in step C, the transverse magnetic field generator applies a transverse static magnetic field of 0.1 to 2 T to the melt.

### Claim 7 (depends on 6)

The method according to claim 6,
wherein in step C, a power of the first heater, the second heater, the third heater, and the fourth heater is adjusted such that a temperatures in a center of the melt in the first temperature area, the second temperature area, the third temperature area, and the fourth temperature area slowly rise by heating in sequence to T1=Tm+(20−100)° C., T2=Tm+20° C., T3=900−1000° C., and T4=600−700° C.;
wherein after the phosphorus bubbles are produced, the temperatures of the melt in the fourth temperature area, the third temperature area, and the second temperature area are gradually increased at a rate of 50-100° C./h until the temperatures of the melt in the fourth temperature area, the third temperature area, and the second temperature area reach T4=Tm+20° C., T3=Tm+20° C., and T2=Tm+(20−100)° C.; and
wherein Tm is the melting point of the synthesized substance.

### Claim 8 (depends on 6)

The method according to claim 6,
wherein in step D, an LEC method or an VFG method is used to grow a crystal.

### Claim 9 (depends on 8)

The method according to claim 8,
wherein after the red phosphorus is completely gasified and no bubbles occur, the temperature of each of the first temperature area, the second temperature area, the third temperature area and the fourth temperature area is adjusted to reach Tm+50° C. and maintain for 20-30 min; the operation of the transverse magnetic field generator is stopped and the temperatures of the first temperature area, the second temperature area, the third temperature area, and the fourth temperature area are adjusted, so that a temperature gradient of 20-100° C./cm is established in the melt from the surface to the bottom; and
wherein pulling starts after the seed crystal contacts the melt, and crystal growth is performed to obtain an LEC crystal.

### Claim 10 (depends on 8)

The method according to claim 8,
wherein a VGF seed crystal is disposed at a bottom of the crucible;
wherein after the red phosphorus is completely gasified and no bubbles occur, the temperature of each of the first temperature area, the second temperature area, the third temperature area and the fourth temperature area is adjusted to reach Tm+50° C. and maintain for 20-30 min;
wherein the operation of the transverse magnetic field generator is stopped and the temperatures of the first temperature area, the second temperature area, the third temperature area, and the fourth temperature area are adjusted, so that a temperature gradient of 3-5° C./cm is established in the melt from the surface to the bottom; and
wherein VGF crystal growth is performed to obtain a VGF crystal.