# US 2024/0308916 A1 · Microwave ferrite material for third-order intermodulation circulator and preparation method therefor

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2024/0308916 A1
- Document ID: US20240308916A1
- Status: Published application
- Kind: A1
- Application number: 18/575,267
- Filed: 2022-08-04
- Published: 2024-09-19
- Earliest claimed: 2021-11-02
- Assignees: Hengdian Group Dmegc Magnetics Co., Ltd
- Applicants: Hengdian Group Dmegc Magnetics Co., Ltd
- Inventors: Feiyu LV; Yuanzhen WANG; Likang ZHANG
- Web page: https://patentgrep.com/patent/US20240308916A1

## CPC

- C04B 35/2641: {Compositions containing one or more ferrites of the group comprising rare earth metals and one or more ferrites of the group comprising alkali metals, alkaline earth metals or lead}
- C04B 35/26: based on ferrites
- C04B 35/6262: {of calcined, sintered clinker or ceramics}
- C04B 35/62625: {Wet mixtures}
- C04B 35/6264: {Mixing media, e.g. organic solvents}
- C04B 35/62645: {Thermal treatment of powders or mixtures thereof other than sintering}
- C04B 35/62655: {Drying, e.g. freeze-drying, spray-drying, microwave or supercritical drying}
- C04B 35/62675: {characterised by the treatment temperature}
- C04B 35/6268: {characterised by the applied pressure or type of atmosphere, e.g. in vacuum, hydrogen or a specific oxygen pressure}
- C04B 35/62685: {characterised by the order of addition of constituents or additives}
- C04B 35/62695: {Granulation or pelletising (devices for shaping artificial aggregates from ceramic mixtures B28B1/004)}
- C04B 35/63416: {Polyvinylalcohols [PVA]; Polyvinylacetates}
- C04B 35/64: Burning or sintering processes (C04B33/32 takes precedence {; powder metallurgy B22F})
- H01F 1/344: {Ferrites, e.g. having a cubic spinel structure (X2+O)(Y23+O3), e.g. magnetite Fe3O4}
- C04B 2235/3212: Calcium phosphates, e.g. hydroxyapatite
- C04B 2235/3225: Yttrium oxide or oxide-forming salts thereof
- C04B 2235/3262: Manganese oxides, manganates, rhenium oxides or oxide-forming salts thereof, e.g. MnO
- C04B 2235/3274: Ferrites
- C04B 2235/3286: Gallium oxides, gallates, indium oxides, indates, thallium oxides, thallates or oxide forming salts thereof, e.g. zinc gallate
- C04B 2235/3293: Tin oxides, stannates or oxide forming salts thereof, e.g. indium tin oxide [ITO]
- C04B 2235/3294: Antimony oxides, antimonates, antimonites or oxide forming salts thereof, indium antimonate
- C04B 2235/3418: Silicon oxide, silicic acids or oxide forming salts thereof, e.g. silica sol, fused silica, silica fume, cristobalite, quartz or flint
- C04B 2235/442: Carbonates
- C04B 2235/5436: micrometer sized, i.e. from 1 to 100 micron
- C04B 2235/5445: submicron sized, i.e. from 0,1 to 1 micron
- C04B 2235/604: Pressing at temperatures other than sintering temperatures
- C04B 2235/606: Drying
- C04B 2235/6562: Heating rate
- C04B 2235/6565: Cooling rate
- C04B 2235/6567: Treatment time
- C04B 2235/6583: Oxygen containing atmosphere, e.g. with changing oxygen pressures
- C04B 2235/6585: at an oxygen percentage above that of air
- H01P 1/38: Circulators
- C04B: LIME, MAGNESIA; SLAG; CEMENTS; COMPOSITIONS THEREOF, e.g. MORTARS, CONCRETE OR LIKE BUILDING MATERIALS; ARTIFICIAL STONE {(roofing granules E04D7/005)}; CERAMICS (devitrified glass-ceramics C03C10/00); REFRACTORIES; TREATMENT OF NATURAL STONE
- H01F: MAGNETS; INDUCTANCES; TRANSFORMERS; SELECTION OF MATERIALS FOR THEIR MAGNETIC PROPERTIES
- H01P: WAVEGUIDES; RESONATORS, LINES, OR OTHER DEVICES OF THE WAVEGUIDE TYPE (operating at optical frequencies G02B)

## Abstract

A microwave ferrite material for a third-order intermodulation circulator and a preparation method therefor, the chemical formula being Y3-aCaaSnaInbMncFe5-a-b-cO12, 0.1≤a≤0.3, 0.01≤b≤0.1, 0.001≤c≤0.1. The preparation method comprises the following steps: (1) weighing; (2) first ball milling; (3) drying and preheating; (4) second ball milling; (5) granulation; and (6) post-treatment. The microwave ferrite material reduces the intermodulation interference between combined signals, and further improves the performance of communication systems and the coverage and capacity of networks. At the same time, it is ensured that the stability and repeatability of the preparation process are maintained at a good level, being suitable for mass production applications.

## Claims

### Claim 1

A microwave ferrite material for a third-order intermodulation circulator, wherein the microwave ferrite material has a chemical formula of Y3-aCaaSnaInbMncFe5-a-b-cO12, wherein 0.1≤a≤0.3, 0.01<b≤0.1, and 0.001≤c≤0.1.

### Claim 2 (depends on 1)

The microwave ferrite material according to claim 1, wherein raw materials of the microwave ferrite material comprise Y2O3, CaCO3, SnO2, In2O3, MnCO3 and Fe2O3.

### Claim 3 (depends on 2)

The microwave ferrite material according to claim 2, wherein the Y2O3 has a purity of more than or equal to 99.95%;
preferably, the CaCO3 has a purity of more than or equal to 99.5%;
preferably, the SnO2 has a purity of more than or equal to 99.5%;
preferably, the In2O3 has a purity of more than or equal to 99.99%;
preferably, the MnCO3 has a purity of more than or equal to 99%;
preferably, the Fe2O3 has a purity of more than or equal to 99.5%.

### Claim 4 (depends on 1)

preparation method for the microwave ferrite material according to claim 1, comprising the following steps:
(1) weighing: weighing out corresponding raw materials according to calculation based on the composition of the microwave ferrite material;
(2) primary ball milling: mixing deionized water, zirconia balls, a dispersant and the raw materials weighed out in step (1), and performing ball milling to obtain a first slurry;
(3) drying and pre-heating: drying and pre-sintering the first slurry obtained in step (2) sequentially to obtain a first powder;
(4) secondary ball milling: mixing deionized water, zirconia balls, a co-solvent and the first powder obtained in step (3), and performing ball milling to obtain a second slurry;
(5) granulation: mixing a binder and the second slurry obtained in step (4), and performing centrifugal spray to obtain a second powder; and
(6) after-treatment: molding, sintering and grinding the second powder obtained in step (5) sequentially to obtain the microwave ferrite material.

### Claim 5 (depends on 4)

The preparation method according to claim 4, wherein the mixing in step (2) has a mass ratio of raw materials: deionized water: zirconia balls=1: (1-1.3):(4-8).

### Claim 6 (depends on 4)

The preparation method according to claim 4, wherein the dispersant in step (2) comprises acetone.

### Claim 7 (depends on 4)

The preparation method according to claim 4, wherein the dispersant in step (2) has a mass proportion of 1-10% in the first slurry.

### Claim 8 (depends on 4)

The preparation method according to claim 4, wherein the ball milling in step (2) has a rotation speed of 60-80 rpm;
preferably, the ball milling in step (2) is carried out for a period of 20-40 h.

### Claim 9 (depends on 4)

The preparation method according to claim 4, wherein the drying in step (3) has a temperature of 120-150° C.;
preferably, the drying in step (3) is carried out for a period of 16-20 h;
preferably, step (3) further comprises screening a powder between the drying and the pre-heating;
preferably, the screening is performed with a mesh size of 40-80 mesh;
preferably, the pre-heating in step (3) has a temperature of 1200-1300° C.;
preferably, the pre-heating in step (3) has a heating rate of 1-2° C./min;
preferably, the pre-heating in step (3) is carried out for a period of 4-8 h;
preferably, the pre-heating in step (3) is performed in an oxygen atmosphere, and oxygen introduction begins when the temperature increases to 800° C., and ends when the temperature decreases to 800° C., and the oxygen introduction has a flow rate of 20-50 L/min.

### Claim 10 (depends on 4)

The preparation method according to claim 4, wherein the mixing in step (4) has a mass ratio of first powder: deionized water: zirconia balls=1: (1-1.3):(4-8);
preferably, the co-solvent in step (4) comprises SiO2;
preferably, the co-solvent in step (4) has a concentration of 50-500 ppm in the second slurry;
preferably, the ball milling in step (4) has a rotation speed of 50-80 rpm;
preferably, the ball milling in step (4) is carried out for a period of 30-50 h.

### Claim 11 (depends on 4)

The preparation method according to claim 4, wherein the binder in step (5) comprises an aqueous solution of polyvinyl alcohol;
preferably, the binder in step (5) has a concentration of 9-11 wt %;
preferably, the binder in step (5) has an addition amount of 8-12 wt %;
preferably, the second powder in step (5) has a particle size X85 of 60-80 μm.

### Claim 12 (depends on 4)

The preparation method according to claim 4, wherein the molding in step (6) is performed with a 100T press.

### Claim 13 (depends on 4)

The preparation method according to claim 4, wherein a cooling stage of the sintering in step (6) comprises two steps, and specifically, the sintered product is firstly cooled to 600° C. at a rate of 1-2° C./min and then cooled naturally;
preferably, the sintering in step (6) is performed in an oxygen atmosphere, and oxygen introduction begins when the temperature increases to 900° C., and ends when the temperature decreases to 700° C., and the oxygen introduction has a flow rate of 30-50 L/min;
preferably, the grinding in step (6) is performed with a centerless grinder.

### Claim 14 (depends on 4)

The preparation method according to claim 4, wherein the preparation method comprises the following steps:
(1) weighing: weighing out corresponding raw materials according to calculation based on the composition of the microwave ferrite material;
(2) primary ball milling: adding the raw materials weighed out in step (1) into a ball milling jar for mixing with a ball mill, feeding materials according to a mass ratio of raw materials: deionized water: zirconia balls=1: (1-1.3):(4-8), adding acetone as a dispersant, and performing ball milling, wherein the ball milling is carried out for a period of 20-40 h with a rotation speed of 60-80 rpm, to obtain a first slurry; the dispersant has a mass proportion of 1-10% in the first slurry, and the first slurry has a particle size X50 of 0.5-1.0 μm;
(3) drying and pre-heating: drying the first slurry obtained in step (2) with an oven, wherein the drying is carried out at a temperature of 120-150° C. for 16-20 h; screening the dried powder with a sieve of 40-80 mesh, and pre-sintering the screened powder with an air sintering furnace, wherein the screened powder is heated to 1200-1300° C. at a rate of 1-2° C./min and held for 4-8 h, to obtain a first powder; the pre-heating is performed in an oxygen atmosphere, and oxygen introduction begins when the temperature increases to 800° C., and ends when the temperature decreases to 800° C., and the oxygen introduction has a flow rate of 20-50 L/min;
(4) secondary ball milling: adding the first powder obtained in step (3) into a ball milling jar for mixing with a ball mill, feeding materials according to a mass ratio of first powder: deionized water: zirconia balls=1: (1-1.3):(4-8), adding SiO2 as a co-solvent, and performing ball milling, wherein the ball milling is carried out for a period of 30-50 h with a rotation speed of 50-80 rpm, to obtain a second slurry; the co-solvent has a concentration of 50-500 ppm in the second slurry, and the second slurry has a particle size X50 of 0.4-0.9 μm;
(5) granulation: adding an aqueous solution of polyvinyl alcohol as a binder at a concentration of 9-11 wt % to the second slurry obtained in step (4), wherein the binder has an addition amount of 8-12 wt %, and performing centrifugal spray to obtain a second powder which has a particle size X85 of 60-80 μm; and
(6) after-treatment: molding, sintering and grinding the second powder obtained in step (5) sequentially to obtain the microwave ferrite material; the molding is performed with a 100T press and yields a cylinder with a density of 3-3.5 g/cm3; a heating stage of the sintering comprises three steps, specifically, a first sintering, a second sintering and a third sintering which are performed sequentially; the first sintering has a temperature of 550-650° C. and a heating rate of 0.5-1.5° C./min; the second sintering has a temperature of 950-1050° C. and a heating rate of 1.5-2.5° C./min; the third sintering has a temperature of 1400-1500° C., a heating rate of 2-3° C./min, and a holding time of 20-40 h; a cooling stage of the sintering comprises two steps, and specifically, the sintered product is firstly cooled to 600° C. at a rate of 1-2° C./min and then cooled naturally; the sintering is performed in an oxygen atmosphere, and oxygen introduction begins when the temperature increases to 900° C., and ends when the temperature decreases to 700° C., and the oxygen introduction has a flow rate of 30-50 L/min; the grinding is performed with a centerless grinder.

### Claim 15

(canceled)

### Claim 16 (depends on 4)

The preparation method according to claim 4, wherein the first slurry in step (2) has a particle size X50 of 0.5-1.0 μm.

### Claim 17 (depends on 4)

The preparation method according to claim 4, wherein the second slurry in step (4) has a particle size X50 of 0.4-0.9 μm.

### Claim 18 (depends on 12)

The preparation method according to claim 12, wherein the first sintering has a temperature of 550-650° C.;
preferably, the first sintering has a heating rate of 0.5-1.5° C./min.

### Claim 19 (depends on 12)

The preparation method according to claim 12, wherein the second sintering has a temperature of 950-1050° C.;
preferably, the second sintering has a heating rate of 1.5-2.5° C./min.

### Claim 20 (depends on 12)

The preparation method according to claim 12, wherein the third sintering has a temperature of 1400-1500° C.;
preferably, the third sintering has a heating rate of 2-3° C./min;
preferably, the third sintering has a holding time of 20-40 h.

### Claim 21 (depends on 1)

A method for manufacturing a third-order intermodulation circulator, comprising using the microwave ferrite material according to claim 1.