# US 2024/0270968 A1 · High-viscosity, high-elasticity, and anti-aging composite modified asphalt and a preparation method thereof

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2024/0270968 A1
- Document ID: US20240270968A1
- Status: Published application
- Kind: A1
- Application number: 18/431,649
- Filed: 2024-02-02
- Published: 2024-08-15
- Earliest claimed: 2023-02-03
- Assignees: Sichuan Road and Bridge Construction Group Co., Ltd.
- Applicants: Sichuan Road and Bridge Construction Group Co., Ltd.
- Inventors: Shuangquan JIANG; Jian YANG; Peilong LI; Wei LU; Liuda CHENG; Yi PEI; Zhan DING; Jianglin DU; Haiqing LI; Jixiang PU; Qingyun LI; Maoqin Niu
- Web page: https://patentgrep.com/patent/US20240270968A1

## CPC

- C08L 95/00: Compositions of bituminous materials, e.g. asphalt, tar, pitch
- C08F 236/08: Isoprene
- C08K 3/06: Sulfur
- C08K 5/12: of cyclic polycarboxylic acids
- C08K 5/3465: condensed with carbocyclic rings
- C08L 9/06: Copolymers with styrene
- C08L 91/00: Compositions of oils, fats or waxes; Compositions of derivatives thereof
- C08L 93/04: Rosin
- C08L 2555/10: Design or test methods for bitumen or asphalt mixtures, e.g. series of measures, procedures or tests to obtain a bitumen or asphalt mixture having preset defined properties, general or international test methods, procedures or standards
- C08L 2555/22: Asphalt produced above 140°C, e.g. hot melt asphalt
- C08L 2555/54: Sulfur or carbon black
- C08L 2555/60: Organic non-macromolecular ingredients, e.g. oil, fat, wax or natural dye
- C08L 2555/80: Macromolecular constituents
- Y02A 30/30: in transportation, e.g. on roads, waterways or railways
- C08L: COMPOSITIONS OF MACROMOLECULAR COMPOUNDS (compositions based on polymerisable monomers C08F, C08G; artificial filaments or fibres D01F; textile treating compositions D06)
- C08F: MACROMOLECULAR COMPOUNDS OBTAINED BY REACTIONS ONLY INVOLVING CARBON-TO-CARBON UNSATURATED BONDS
- C08K: Use of inorganic or non-macromolecular organic substances as compounding ingredients (paints, inks, varnishes, dyes, polishes, adhesives C09)
- Y02A: TECHNOLOGIES FOR ADAPTATION TO CLIMATE CHANGE

## Abstract

The disclosure discloses a high-viscosity, high-elasticity, and anti-aging composite modified asphalt and a preparation method thereof, solves the technical problem that the comprehensive performance of an existing asphalt ultrathin wearing layer needs to be further improved so as to prolong the service life of a pavement surface layer and reduce the pavement maintenance costs. The composite modified asphalt is prepared from the following components in parts by mass: 100 parts of a matrix asphalt, 10 to 15 parts of a thermoplastic styrene-butadiene rubber, 5 to 8 parts of a tackifier, 0.5 to 1.5 parts of a plasticizer, 2 to 5 parts of a compatilizer, 0.1 to 0.4 parts of a stabilizer, and 0.01 to 0.05 parts of an anti-aging agent. The composite modified asphalt prepared by the disclosure has the advantages of high elasticity, high viscosity, excellent aging resistance, etc.

## Claims

### Claim 1

A high-viscosity, high-elasticity, and anti-aging composite modified asphalt, characterized by, according to parts by mass, comprising the following components:
100 parts of a matrix asphalt, 12 parts of a thermoplastic styrene-butadiene rubber, 7 parts of a tackifier, 1 part of a plasticizer, 3 parts of a compatilizer, 0.25 parts of a stabilizer, and 0.05 parts of an anti-aging agent,
the tackifier is a compound of a resin and a polyisoprene derivative, and the resin is a rosin modified resin, the structural formula of the polyisoprene derivative is:
the mass ratio of the resin to the polyisoprene derivative is 2:1,
the thermoplastic styrene-butadiene rubber has a linear structure, and has a block ratio S/B of 30/70,
the plasticizer is dioctyl phthalate, the compatilizer is an extract oil from furfural refining, the stabilizer is sulfur, and the anti-aging agent is 9,9-dimethylacridine,
the high-viscosity, high-elasticity, and anti-aging composite modified asphalt is prepared by the following method:
step 1: melting a matrix asphalt and maintaining the temperature, adding weighed plasticizer, compatilizer and anti-aging agent to the molten asphalt, and dispersing evenly;
step 2: adding a thermoplastic styrene-butadiene rubber to the asphalt obtained in the step 1, swelling, then heating up, and shearing at a high speed to completely dissolve the thermoplastic elastomer in the asphalt;
the specific method of the step 2 comprises: adding the weighed thermoplastic styrene-butadiene rubber to the asphalt obtained in step 1, stirring, swelling for 10 min, then heating the asphalt to 180±5° C., and shearing at a high speed of 4500-5500 r/min for 20-40 min to completely dissolve the thermoplastic elastomer in the asphalt;
step 3: adding a tackifier to the asphalt obtained in the step 2, adding a stabilizer after high-speed shearing, and then shearing for stable crosslinking; and
step 4: developing the asphalt obtained in the step 3, and regularly removing gas, so as to obtain a high-viscosity, high-elasticity, high-performance, and anti-aging composite modified asphalt;
the specific step of the step 4 comprises: after shearing is completed, transferring a modified asphalt sample into an oven at 170-180° C. for development for 45 minutes, and stirring the asphalt sample every 10-15 minutes to discharge the air mixed in the asphalt, so as to obtain a high-viscosity, high-elasticity, high-performance, and anti-aging composite modified asphalt;
The high-viscosity, high performance, aging resistant composite modified asphalt has a dynamic viscosity of 253248 at 60° C., a needle penetration at 25° C. of 51.2, a ductility at 25° C. of 42.5 cm, a softening point of 96.4° C., a storage stability of 1.5° C. of 48 h, a residual needle penetration at 25° C. of 79% after RTFOT, and a residual ductility at 5° C. of 34 cm.

### Claim 2 (depends on 1)

A preparation method for a high-viscosity, high-elasticity, and anti-aging composite modified asphalt, characterized in that the preparation method is used for preparing the composite modified asphalt of claim 1, and comprises the following steps:
step 1: melting a matrix asphalt and maintaining the temperature, adding weighed plasticizer, compatilizer and anti-aging agent to the molten asphalt, and dispersing evenly;
step 2: adding a thermoplastic styrene-butadiene rubber to the asphalt obtained in the step 1, swelling, then heating up, and shearing at a high speed to completely dissolve the thermoplastic elastomer in the asphalt;
step 3: adding a tackifier to the asphalt obtained in the step 2, adding a stabilizer after high-speed shearing, and then shearing for stable crosslinking; and
step 4: developing the asphalt obtained in the step 3, and regularly removing gas, so as to obtain a high-viscosity, high-elasticity, high-performance, and anti-aging composite modified asphalt.

### Claim 3 (depends on 2)

The preparation method for a high-viscosity, high-elasticity, and anti-aging composite modified asphalt according to claim 2, wherein the specific method of the step 1 comprises: firstly, placing the matrix asphalt into an oven at 125-145° C. to completely melt the matrix asphalt, then maintaining the temperature of the matrix asphalt at 145-155° C. in an electric heating mantle, adding the weighed plasticizer, compatilizer and anti-aging agent into the melted asphalt, and stirring to make same evenly dispersed in the matrix asphalt.

### Claim 4 (depends on 2)

The preparation method for a high-viscosity, high-elasticity, and anti-aging composite modified asphalt according to claim 2, wherein the specific method of the step 2 comprises: adding the weighed thermoplastic styrene-butadiene rubber to the asphalt obtained in step 1, stirring, swelling for 10-15 min, then heating the asphalt to 180±5° C., and shearing at a high speed of 4500-5500 r/min for 20-40 min to completely dissolve the thermoplastic elastomer in the asphalt.

### Claim 5 (depends on 2)

The preparation method for a high-viscosity, high-elasticity, and anti-aging composite modified asphalt according to claim 2, wherein the specific method of said step 3 comprises: adding weighed tackifier, shearing at a rotating speed of 4000-5000 r/min for 15-30 min, finally adding weighed sulfur, and shearing at a rotating speed of 3500-4000 r/min for 10-20 min for stable cross-linking.

### Claim 6 (depends on 2)

The preparation method for a high-viscosity, high-elasticity, and anti-aging composite modified asphalt according to claim 2, wherein the specific step of the step 4 comprises: after shearing is completed, transferring a modified asphalt sample into an oven at 170-180° C. for development for 45 minutes, and stirring the asphalt sample every 10-15 minutes to discharge the air mixed in the asphalt, so as to obtain a high-viscosity, high-elasticity, high-performance, and anti-aging composite modified asphalt.

### Claim 7 (depends on 3)

The preparation method for a high-viscosity, high-elasticity, and anti-aging composite modified asphalt according to claim 3, wherein the specific method of the step 2 comprises: adding the weighed thermoplastic styrene-butadiene rubber to the asphalt obtained in step 1, stirring, swelling for 10-15 min, then heating the asphalt to 180±5° C., and shearing at a high speed of 4500-5500 r/min for 20-40 min to completely dissolve the thermoplastic elastomer in the asphalt.

### Claim 8 (depends on 3)

The preparation method for a high-viscosity, high-elasticity, and anti-aging composite modified asphalt according to claim 3, wherein the specific method of said step 3 comprises: adding weighed tackifier, shearing at a rotating speed of 4000-5000 r/min for 15-30 min, finally adding weighed sulfur, and shearing at a rotating speed of 3500-4000 r/min for 10-20 min for stable cross-linking.

### Claim 9 (depends on 3)

The preparation method for a high-viscosity, high-elasticity, and anti-aging composite modified asphalt according to claim 3, wherein the specific step of the step 4 comprises: after shearing is completed, transferring a modified asphalt sample into an oven at 170-180° C. for development for 45 minutes, and stirring the asphalt sample every 10-15 minutes to discharge the air mixed in the asphalt, so as to obtain a high-viscosity, high-elasticity, high-performance, and anti-aging composite modified asphalt.