# US 2024/0269734 A1 · Method for producing a microalloyed steel, a microalloyed steel produced using the method, and a combined casting/rolling installation

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2024/0269734 A1
- Document ID: US20240269734A1
- Status: Published application
- Kind: A1
- Application number: 18/568,741
- Filed: 2022-05-25
- Published: 2024-08-15
- Earliest claimed: 2021-06-09
- Assignees: Primetals Technologies Austria GmbH
- Applicants: Primetals Technologies Austria GmbH
- Inventors: Kerstin BAUMGARTNER; Simon GROSSEIBER; Thomas LENGAUER; Gero SCHWARZ
- Web page: https://patentgrep.com/patent/US20240269734A1

## CPC

- B22D 11/001: {of specific alloys}
- C22C 38/12: containing tungsten, tantalum, molybdenum, vanadium, or niobium
- B22D 11/0408: {Moulds for casting thin slabs}
- B22D 11/1206: {for plastic shaping of strands (rolling mills B21B1/46)}
- B22D 11/124: for cooling
- B22D 11/225: {for secondary cooling}
- C21D 1/667: for spray quenching
- C21D 8/0215: {Rapid solidification; Thin strip casting}
- C21D 8/0226: {Hot rolling}
- C21D 8/0263: {following hot rolling}
- C21D 9/46: for sheet metals
- C21D 9/573: with cooling
- C21D 9/5737: {Rolls; Drums; Roll arrangements}
- C21D 11/005: {for cooling}
- C22C 38/001: {containing N}
- C22C 38/02: containing silicon
- C22C 38/04: containing manganese
- C22C 38/16: containing copper
- C22C 38/22: with molybdenum or tungsten
- C22C 38/24: with vanadium
- C22C 38/26: with niobium or tantalum
- C22C 38/28: with titanium or zirconium
- C22C 38/44: with molybdenum or tungsten
- C22C 38/46: with vanadium
- C22C 38/48: with niobium or tantalum
- C22C 38/50: with titanium or zirconium
- B21B 1/463: {in a continuous process, i.e. the cast not being cut before rolling}
- C21D 1/42: Induction heating
- C21D 9/60: with induction heating
- C21D 2211/004: Dispersions; Precipitations
- C21D 2261/00: Machining or cutting being involved
- B22D: CASTING OF METALS; CASTING OF OTHER SUBSTANCES BY THE SAME PROCESSES OR DEVICES (shaping of plastics or substances in a plastic state B29C; metallurgical processing, selection of substances to be added to metal C21, C22)
- C22C: ALLOYS (treatment of alloys C21D, C22F)
- C21D: MODIFYING THE PHYSICAL STRUCTURE OF FERROUS METALS; GENERAL DEVICES FOR HEAT TREATMENT OF FERROUS OR NON-FERROUS METALS OR ALLOYS; MAKING METAL MALLEABLE, e.g. BY DECARBURISATION OR TEMPERING (surface treatment of metallic material involving at least one process provided for in class C23 and at least one process covered by this subclass C23F17/00; unidirectional solidification of eutectic materials or unidirectional demixing of eutectoid materials C30B)
- B21B: ROLLING OF METAL (auxiliary operations used in connection with metal-working operations covered in B21, see B21C; bending by rolling B21D; manufacture of particular objects, e.g. screws, wheels, rings, barrels, balls, by rolling B21H; pressure welding by means of a rolling mill B23K20/04)

## Abstract

A process that produces a microalloyed steel in an integrated casting-rolling plant having a continuous casting machine with a mold, a single- or multi-stand prerolling train, a finish-rolling train having a first stand group with at least one first finish-rolling stand and a second stand group having at least one stand cooler. A metallic melt is cast in the mold to obtain a partly solidified thin-slab strand, which is supported, deflected and cooled. The solidified thin-slab strand is rolled by the prerolling train to obtain a prerolled strip that is finish-rolled in the first stand group to obtain the finish-rolled strip, which is fed to the second stand group and force-cooled in the second stand group, the finish-rolled strip having a thickness that results in a cooling rate of the core of the finish-rolled strip in the second stand group greater than 20° C./s and less than 200° C./s.

## Claims

### Claim 1

A process for producing a microalloyed steel in an integrated casting-rolling plant, preferably in continuous operation,
wherein the integrated casting-rolling plant has a continuous casting machine having a mold, a single- or multi-stand prerolling train, a finish-rolling train having a first stand group with at least one first finish-rolling stand and a second stand group having at least one stand cooler,
wherein a metallic melt is cast in the mold to give a partly solidified thin-slab strand,
wherein the partly solidified thin-slab strand is supported, deflected and cooled,
wherein the prerolling train rolls the fully solidified thin-slab strand to give a prerolled strip,
wherein the first stand group of the finish-rolling train finish-rolls the prerolled strip to give the finish-rolled strip,
wherein, immediately after the finish rolling, the finish-rolled strip is fed to the second stand group and the finish-rolled strip is force-cooled in the second stand group with retention of a thickness of the finish-rolled strip in such a way that a cooling rate of a core of the finish-rolled strip in the second stand group is greater than 20° C./s and less than 200° C./s.

### Claim 2 (depends on 1)

The process as claimed in claim 1,
wherein the second stand group has a second finish-rolling stand,
wherein the second finish-rolling stand, in a preparation step prior to casting of the metallic melt, is converted to the stand cooler by removing at least one working roll of the second finish-rolling stand and inserting at least one cooling beam into the second finish-rolling stand.

### Claim 3 (depends on 1)

The process as claimed in claim 1,
wherein a third surface temperature with which the finish-rolled strip leaves the second stand group is ascertained,
wherein the forced cooling in the second stand group is controlled by open-loop/closed-loop control depending on the third surface temperature and a third target temperature (TS3) in such a way that the third surface temperature corresponds essentially to the third target temperature (TS3),
wherein the third target temperature (TS3) is less than a ferrite-perlite transformation temperature (Ar1), preferably less than a bainite start temperature, especially less than a martensite start temperature (Ms).

### Claim 4 (depends on 3)

The process as claimed in claim 3,
wherein a second surface temperature with which the finish-rolled strip leaves the first stand group is ascertained,
wherein the second surface temperature is also taken into account in the control of the forced cooling of the finish-rolled strip in the second stand group.

### Claim 5 (depends on 1)

The process as claimed in claim 1,
wherein the cooling rate of the core of the finish-rolled strip is 20° C./s to 80° C./s, especially 45° C./s to 55° C./s,
wherein the core of the finish-rolled strip is preferably cooled continuously.

### Claim 6 (depends on 1)

The process as claimed in claim 1,
wherein the core of the finish-rolled strip is transported with a first exit temperature (TA1) of 830° C. to 950° C., especially of 880° C. to 920° C., into the second stand group of the finish-rolling train,
wherein, on exit of the finish-rolled strip from the second stand group, the core of the finish-rolled strip has a second exit temperature (TA2) of less than 700° C., especially 350° C. to 700° C., preferably of 400° C. to 460° C.

### Claim 7 (depends on 5)

The process as claimed in claim 5,
wherein the core of the finish-rolled strip is cooled, preferably continuously, from the first exit temperature (TA1) to the second exit temperature (TA2) within a time interval of 2 seconds to 40 seconds.

### Claim 8 (depends on 1)

The process as claimed in claim 1,
wherein, within a time interval of 1 second to 15 seconds after the finish-rolling of the finish-rolled strip in the first stand group, the finish-rolled strip enters the second stand group.

### Claim 9 (depends on 1)

The process as claimed in claim 1,
wherein the integrated casting-rolling plant has a cooling zone downstream of the finish-rolling train based on a conveying direction of the finish-rolled strip and a winding device downstream of the cooling zone,
wherein forced cooling of the finish-rolled strip in the cooling zone is deactivated and the finish-rolled strip is transported through the cooling zone from the second stand group to the winding device.

### Claim 10 (depends on 1)

The process as claimed in claim 1,
wherein a thickness of the prerolled strip on entry into the first stand group is 40 mm to 62 mm, especially 45 mm,
wherein the first stand group reduces the thickness of the prerolled strip to that of the finish-rolled strip of 10 mm to 25 mm, especially 16 mm to 20 mm.

### Claim 11 (depends on 1)

The process as claimed in claim 1,
wherein the metallic melt for an X60 or an X70 steel has a chemical composition in percent by weight of C 0.025-0.05%; Si 0.1-0.3%; Mn 0.07-1.5%, Cr<0.15%; Mo<0.2%; Nb 0.02-0.08%; Ti<0.05%; V<0.08%; N<0.008%; balance: Fe and unavoidable impurities, or
wherein the metallic melt for X80 to X120 steels, especially for X90 to X120 steels, has a chemical composition in percent by weight of C 0.025-0.09%; Si 0.1-0.3%; Mn 0.07-2.0%, Cr<0.5%; Mo<0.5%; Nb 0.02-0.08%; Ti<0.05%; V<0.08%; Ni<0.5%; Cu<0.4%; N<0.01%; balance: Fe and unavoidable impurities.

### Claim 12 (depends on 1)

A microalloyed steel, especially microalloyed piping steel having a thickness of 10 mm to 25 mm, especially of 16 mm to 20 mm, produced by a process as claimed in claim 1,
having a chemical composition for an X60 or an X70 steel in percent by weight of C 0.025-0.05%; Si 0.1-0.3%; Mn 0.07-1.5%, Cr<0.15%; Mo<0.2%; Nb 0.02-0.08%; Ti<0.05%; V<0.08%; N<0.008%; balance: Fe and unavoidable impurities
or
having a chemical composition for an X80 to X120 steel in percent by weight of C 0.025-0.09%; Si 0.1-0.3%; Mn 0.07-2.0%, Cr<0.5%; Mo<0.5%; Nb 0.02-0.08%; Ti<0.05%; V<0.08%; Ni<0.5%; Cu<0.4%; N<0.01%; balance: Fe and unavoidable impurities.

### Claim 13 (depends on 12)

The microalloyed steel as claimed in claim 12,
wherein the microalloyed steel at room temperature has at least one of the following precipitates: Ti(C,N), Nb(C,N) V(C,N) TiC, TIN, Ti(C,N), (Nb,Ti)C, (Nb,Ti)N, (Nb,Ti)(C,N), NbC, NbN, VC, VN, V(C,N), (Nb,Ti,V)(C,N), (Nb,V)C, (Ti,V)C, (Nb,V)(C,N), (Ti,V)(C,N), (Nb,V)N, (Ti,V)N, (Nb,Ti,V)C, (Nb,Ti,V)N,
wherein a precipitate density of the precipitates is preferably 1020-1023 1/m3,
wherein the precipitates preferably have an average size of 1 nm to 15 nm,
wherein the precipitate density and/or the average size is determinable by transmission electron microscopy,
wherein a precipitate size, for determination of the average size of the precipitates, should be determined transverse to a conveying direction of the finish-rolled strip and at right angles to a cross section of the finish-rolled strip.

### Claim 14 (depends on 1)

An integrated casting-rolling plant for production of a microalloyed steel by a process as claimed in claim 1,
having a continuous casting machine having a mold, a single- or multi-stand prerolling train, and a finish-rolling train having at least a first stand group and a second stand group,
where in a metallic melt is castable in the mold to give a partly solidified thin-slab strand and the thin-slab strand is feedable to the prerolling train,
wherein the prerolling train is designed to roll the fully solidified thin-slab strand to a prerolled strip,
wherein the finish-rolling train is feedable with the prerolled strip and the first stand group is designed to finish-roll the prerolled strip to a finish-rolled strip,
wherein, based on a conveying direction of the finish-rolled strip, the second stand group is downstream of the first stand group and has at least one stand cooler,
wherein the second stand group is designed, with retention of a thickness of the finish-rolled strip, to force-cool the finish-rolled strip in such a way that a cooling rate of a core of the finish-rolled strip in the second stand group is greater than 20° C./s and less than 200° C./s.

### Claim 15 (depends on 14)

The integrated casting-rolling plant as claimed in claim 14,
having a cooling zone downstream of the second stand group based on the conveying direction of the finish-rolled strip; and a winding device downstream of the cooling zone,
wherein, on forced cooling of the finish-rolled strip in the second stand group, forced cooling of the finish-rolled strip in the cooling zone is deactivated and the cooling zone is designed exclusively to transport the finish-rolled strip to the winding device,
wherein the integrated casting-rolling plant preferably has a third temperature measurement device and a control unit,
wherein the third temperature measurement device and the second stand group preferably have a data connection to the control unit,
wherein the third temperature measurement device, based on the conveying direction of the finish-rolled strip, is preferably disposed between the second stand group and the cooling zone and is designed to ascertain a third surface temperature of the finish-rolled strip,
wherein the control unit is preferably designed, on the basis of the ascertained third surface temperature of the finish-rolled strip and a predefined third target temperature (TS3), to control the forced cooling of the second stand group.