# US 2024/0254582 A1 · Hot-rolled steel plate having excellent impact toughness of welded zone and method for manufacturing same

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2024/0254582 A1
- Document ID: US20240254582A1
- Status: Published application
- Kind: A1
- Application number: 18/019,183
- Filed: 2021-08-11
- Published: 2024-08-01
- Earliest claimed: 2020-08-26
- Assignees: Posco
- Applicants: POSCO Co., Ltd
- Inventors: Wan-Keun Kim; Duk-Gyu Kim
- Web page: https://patentgrep.com/patent/US20240254582A1

## CPC

- C22C 38/002: {containing In, Mg, or other elements not provided for in one single group C22C38/001 - C22C38/60}
- C21D 1/02: Hardening articles or materials formed by forging or rolling, with no further heating beyond that required for the formation
- C21D 6/005: {containing Mn}
- C21D 8/0226: {Hot rolling}
- C21D 8/0263: {following hot rolling}
- C21D 9/46: for sheet metals
- C22C 38/001: {containing N}
- C22C 38/02: containing silicon
- C22C 38/04: containing manganese
- C22C 38/06: containing aluminium
- C22C 38/08: containing nickel {(C22C38/105 takes precedence)}
- C22C 38/12: containing tungsten, tantalum, molybdenum, vanadium, or niobium
- C22C 38/14: containing titanium or zirconium
- C22C 38/16: containing copper
- C22C 38/42: with copper
- C22C 38/44: with molybdenum or tungsten
- C22C 38/48: with niobium or tantalum
- C22C 38/50: with titanium or zirconium
- C21D 2211/002: Bainite
- C21D 2211/005: Ferrite
- C21D 2211/009: Pearlite
- C22C: ALLOYS (treatment of alloys C21D, C22F)
- C21D: MODIFYING THE PHYSICAL STRUCTURE OF FERROUS METALS; GENERAL DEVICES FOR HEAT TREATMENT OF FERROUS OR NON-FERROUS METALS OR ALLOYS; MAKING METAL MALLEABLE, e.g. BY DECARBURISATION OR TEMPERING (surface treatment of metallic material involving at least one process provided for in class C23 and at least one process covered by this subclass C23F17/00; unidirectional solidification of eutectic materials or unidirectional demixing of eutectoid materials C30B)

## Abstract

The present invention relates to a steel sheet suitable as a material for transporting oil and gas, more particularly, to a hot-rolled steel sheet having excellent impact toughness in a welded zone after electric resistance welding (ERW), and to a hot-rolled steel sheet having excellent impact toughness at a cryogenic temperature of −20° C. or lower, that makes the sheet applied in a cold area, and a method for manufacturing same.

## Claims

### Claim 1

A hot-rolled steel sheet having excellent impact toughness in a welded zone, comprising, by weight: 0.02 to 0.05% of carbon (C), 0.05 to 0.3% of silicon (Si), 0.4 to 1.2% of manganese (Mn), 0.01% or less of phosphorus (P) (excluding 0%), 0.001% or less of sulfur (S) (excluding 0%), 0.02 to 0.05% of aluminum (Al), 0.02 to 0.06% of niobium (Nb), 0.05 to 0.3% of nickel (Ni), 0.005 to 0.03% of titanium (Ti), 0.002 to 0.008% of nitrogen (N), and 0.0015 to 0.004% of calcium (Ca), with a balance of Fe and other unavoidable impurities,
wherein the steel sheet satisfies the following Relation 1 and includes polygonal ferrite in an area fraction of 35% or more (less than 100%) as a microstructure, and the crystal grain average size of high angle grains having 15° or more as measured by EBSD is 15 μm or less:
3≤Mn/Si≤5 (Relation 1)
wherein Mn and Si refer to a weight content, respectively.

### Claim 2 (depends on 1)

The hot-rolled steel sheet having excellent impact toughness in a welded zone of claim 1, further optionally comprising: at least one of copper (Cu), chromium (Cr), molybdenum (Mo), and vanadium (V), a total content thereof being 1.0% or less.

### Claim 3 (depends on 1)

The hot-rolled steel sheet of claim 1 having excellent impact toughness in a welded zone, wherein the hot-rolled steel sheet includes one or more of acicular ferrite, bainite, and pearlite as a residual structure other than the polygonal ferrite.

### Claim 4 (depends on 1)

The hot-rolled steel sheet of claim 1 having excellent impact toughness in a welded zone, wherein the hot-rolled steel sheet has a yield strength of 300 to 600 MPa.

### Claim 5 (depends on 1)

The hot-rolled steel sheet of claim 1 having excellent impact toughness in a welded zone, wherein an impact energy value of the welded zone after welding the hot-rolled steel sheet by an electric resistance welding (ERW) method is 50 J or more at −30° C.

### Claim 6

A method for manufacturing a hot-rolled steel sheet having excellent impact toughness in a welded zone, the method comprising:
preparing a steel slab which includes, by weight: 0.02 to 0.05% of carbon (C), 0.05 to 0.3% of silicon (Si), 0.4 to 1.2% of manganese (Mn), 0.01% or less of phosphorus (P) (excluding 0%), 0.001% or less of sulfur (S) (excluding 0%), 0.02 to 0.05% of aluminum (Al), 0.02 to 0.06% of niobium (Nb), 0.05 to 0.3% of nickel (Ni), 0.005 to 0.03% of titanium (Ti), 0.002 to 0.008% of nitrogen (N), and 0.0015 to 0.004% of calcium (Ca), with a balance of Fe and other unavoidable impurities, and satisfies the following Relation 1;
heating the steel slab in a temperature range of 1150 to 1300° C.;
finish hot rolling the heated steel slab in a temperature range of Ar3 to 950° C.;
after the finish hot rolling, performing cooling to a temperature range of 400 to 650° C. at a cooling rate of 10° C./s or more; and
after the cooling, performing coiling:
3≤Mn/Si≤5 (Relation 1)
wherein Mn and Si refer to a weight content, respectively.

### Claim 7 (depends on 6)

The method for manufacturing a hot-rolled steel sheet having excellent impact toughness in a welded zone of claim 6, wherein the finish hot rolling is performed to a cumulative reduction rate of 70% or more.

### Claim 8 (depends on 6)

The method for manufacturing a hot-rolled steel sheet having excellent impact toughness in a welded zone of claim 6, wherein the cooling is started at Ar3 or higher immediately after the finish hot rolling.

### Claim 9 (depends on 6)

The method for manufacturing a hot-rolled steel sheet having excellent impact toughness in a welded zone of claim 6, wherein the steel slab further optionally includes at least one of copper (Cu), chromium (Cr), molybdenum (Mo), and vanadium (V), a total content thereof being 1.0% or less.