# US 2024/0247350 A1 · Seamless steel tube resistant to carbon dioxide corrosion and manufacturing method therefor

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2024/0247350 A1
- Document ID: US20240247350A1
- Status: Published application
- Kind: A1
- Application number: 18/290,401
- Filed: 2022-05-20
- Published: 2024-07-25
- Earliest claimed: 2021-05-21
- Assignees: Baoshan Iron & Steel Co., Ltd.
- Applicants: Baoshan Iron & Steel Co., Ltd.
- Inventors: Suzhen Luo; Yameng Qi; Zhonghua Zhang
- Web page: https://patentgrep.com/patent/US20240247350A1

## CPC

- C22C 38/22: with molybdenum or tungsten
- B21B 19/04: Rolling basic material of solid, i.e. non-hollow, structure; Piercing {, e.g. rotary piercing mills}
- B21C 37/06: of tubes or metal hoses; Combined procedures for making tubes, e.g. for making multi-wall tubes
- C21D 1/25: Hardening, combined with annealing between 300 degrees Celsius and 600 degrees Celsius, i.e. heat refining ("Vergüten")
- C21D 6/002: {containing Cr (C21D6/004 takes precedence)}
- C21D 6/004: {containing Cr and Ni}
- C21D 6/008: {containing Si}
- C21D 8/10: during manufacturing of tubular bodies
- C21D 9/08: for tubular bodies or pipes
- C21D 9/085: {Cooling or quenching}
- C22C 33/04: by melting
- C22C 38/001: {containing N}
- C22C 38/002: {containing In, Mg, or other elements not provided for in one single group C22C38/001 - C22C38/60}
- C22C 38/005: {containing rare earths, i.e. Sc, Y, Lanthanides}
- C22C 38/02: containing silicon
- C22C 38/04: containing manganese
- C22C 38/06: containing aluminium
- C22C 38/18: containing chromium
- C22C 38/24: with vanadium
- C22C 38/26: with niobium or tantalum
- C22C 38/28: with titanium or zirconium
- C22C 38/32: with boron
- C22C 38/44: with molybdenum or tungsten
- C22C 38/48: with niobium or tantalum
- C22C 38/50: with titanium or zirconium
- C22C 38/54: with boron
- B21B 2267/12: Roll temperature
- C22C: ALLOYS (treatment of alloys C21D, C22F)
- B21B: ROLLING OF METAL (auxiliary operations used in connection with metal-working operations covered in B21, see B21C; bending by rolling B21D; manufacture of particular objects, e.g. screws, wheels, rings, barrels, balls, by rolling B21H; pressure welding by means of a rolling mill B23K20/04)
- B21C: MANUFACTURE OF METAL SHEETS, WIRE, RODS, TUBES, PROFILES OR LIKE SEMI-MANUFACTURED PRODUCTS OTHERWISE THAN BY ROLLING; AUXILIARY OPERATIONS USED IN CONNECTION WITH METAL-WORKING WITHOUT ESSENTIALLY REMOVING MATERIAL
- C21D: MODIFYING THE PHYSICAL STRUCTURE OF FERROUS METALS; GENERAL DEVICES FOR HEAT TREATMENT OF FERROUS OR NON-FERROUS METALS OR ALLOYS; MAKING METAL MALLEABLE, e.g. BY DECARBURISATION OR TEMPERING (surface treatment of metallic material involving at least one process provided for in class C23 and at least one process covered by this subclass C23F17/00; unidirectional solidification of eutectic materials or unidirectional demixing of eutectoid materials C30B)

## Abstract

Disclosed in the present application is a high-strength seamless steel tube resistant to carbon dioxide corrosion. In addition to containing Fe and inevitable impurities, the seamless steel tube comprises the following chemical elements in mass percentage: C: 0.05-0.18%, Si: 0.15-0.40%, Mn: 0.25-0.50%, Cr: 4.0-6.0%, Mo: 0.08-0.35%, Al: 0.020-0.055%, Ca: 0.001-0.004%; and one or more elements selected from Ti, Nb, V, Ce, and La, wherein 0.003%≤Ti+Nb+V+Ce+La≤0.20%. Also disclosed in the present application is a manufacturing method for the seamless steel tube. The method comprises the following steps: (1) manufacturing a tube billet; (2) subjecting the tube billet to heating, perforating, hot rolling, and sizing to obtain a hot-rolled tube; and (3) subjecting the hot-rolled tube to a quenching and tempering heat treatment: quenching within a temperature range of 860-940° C. for 15-120 min, and then tempering within a temperature range of 520-620° C. for 30-150 min.

## Claims

### Claim 1

A seamless steel tube resistant to corrosion by carbon dioxide, comprising the following chemical elements in mass percentage, in addition to containing Fe and inevitable impurities:
C: 0.05-0.18%, Si: 0.15-0.40%, Mn: 0.25-0.50%, Cr: 4.0-6.0%, Mo: 0.08-0.35%, Al: 0.020-0.055%, Ca: 0.001-0.004%; and one or more selected from Ti, Nb, V, Ce, and La, wherein 0.003%≤Ti+Nb+V+Ce+La≤0.20%.

### Claim 2 (depends on 1)

The seamless steel tube according to claim 1, wherein the seamless steel tube consists of the following chemical elements in mass percentage:
C: 0.05-0.18%, Si: 0.15-0.40%, Mn: 0.25-0.50%, Cr: 4.0-6.0%, Mo: 0.08-0.35%, Al: 0.020-0.055%, Ca: 0.001-0.004%; and one or more selected from Ti, Nb, V, Ce, and La, wherein 0.003%≤Ti+Nb+V+Ce+La≤0.20%, and the balance of Fe and inevitable impurities.

### Claim 3 (depends on 1)

The seamless steel tube according to claim 1, wherein the content of the chemical elements in the seamless steel tube further satisfy at least one of the following:
C: 0.09-0.15%,
Si: 0.2-0.35%,
Mn: 0.3-0.45%,
Cr: 4.5-5.5%,
Mo: 0.1-0.25%,
Al: 0.025-0.045%,
Ca: 0.0015-0.003%, and
0.005%≤Ti+Nb+V+Ce+La≤0.15%.

### Claim 4 (depends on 1)

The seamless steel tube according to claim 1, wherein among the inevitable impurities, P≤0.015%, S≤0.008%, N≤0.006%, and O≤0.0035%.

### Claim 5 (depends on 4)

The seamless steel tube according to claim 4, wherein among the inevitable impurities, P≤0.012%, S≤0.005%, N≤0.0045%, and O≤0.002%.

### Claim 6 (depends on 1)

The seamless steel tube according to claim 1, having a tempered sorbite structure.

### Claim 7 (depends on 1)

The seamless steel tube according to claim 1, wherein the properties of the seamless steel tube satisfy at least one of the following:
yield strength Rp0.2≥550 MPa, tensile strength Rm≥670 MPa, elongation A50≥15%, and impact property KV8≥60 J;
under the dynamic corrosion environment conditions of 60-90° C., 0.5 MPa CO2, 50,000 ppm Cl−, and 1 m/s, a weight loss corrosion rate is less than 0.08 mm/d, and a pitting corrosion rate is less than 0.2 mm/d.

### Claim 8 (depends on 1)

A manufacturing method for the seamless steel tube resistant to carbon dioxide corrosion according to claim 1, wherein the manufacturing method excludes a spheroidizing annealing step and comprises the following steps:
(1) manufacturing a tube billet;
(2) subjecting the tube billet to heating, perforating, hot rolling, and sizing to obtain a hot-rolled tube; and
(3) subjecting the hot-rolled tube to quenching and tempering heat treatment: quenching the hot-rolled tube in a temperature range of 860-940° C. and holding for 15-120 min, followed by tempering the quenching tube in a temperature range of 520-620° C. and holding for 30-150 min.

### Claim 9 (depends on 8)

The manufacturing method according to claim 8, wherein in the heating step of step (2), the tube billet is heated at 1180-1280° C. and held for 120-350 min.

### Claim 10 (depends on 8, 9)

The manufacturing method according to claim 8 or 9, wherein in step (2), perforating, hot rolling, and sizing are performed in a temperature range of 1160-1260° C.

### Claim 11 (depends on 2)

The seamless steel tube according to claim 2, wherein the content of the chemical elements in the seamless steel tube further satisfy at least one of the following:
C: 0.09-0.15%,
Si: 0.2-0.35%,
Mn: 0.3-0.45%,
Cr: 4.5-5.5%,
Mo: 0.1-0.25%,
Al: 0.025-0.045%,
Ca: 0.0015-0.003%, and
0.005%≤Ti+Nb+V+Ce+La≤0.15%.

### Claim 12 (depends on 2)

The seamless steel tube according to claim 2, wherein among the inevitable impurities, P≤0.015%, S≤0.008%, N≤0.006%, and O≤0.0035%.

### Claim 13 (depends on 2)

The seamless steel tube according to claim 2, having a tempered sorbite structure.

### Claim 14 (depends on 2)

The seamless steel tube according to claim 2, wherein the properties of the seamless steel tube satisfy at least one of the following:
yield strength Rp0.2≥550 MPa, tensile strength Rm≥670 MPa, elongation A50≥15%, and impact property KV8≥60 J;
under the dynamic corrosion environment conditions of 60-90° C., 0.5 MPa CO2, 50,000 ppm Cl−, and 1 m/s, a weight loss corrosion rate is less than 0.08 mm/d, and a pitting corrosion rate is less than 0.2 mm/d.

### Claim 15 (depends on 9)

The manufacturing method according to claim 9, wherein in step (2), perforating, hot rolling, and sizing are performed in a temperature range of 1160-1260° C.