# US 2024/0239024 A1 · Mold release for engineered stone and other mold release applications

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2024/0239024 A1
- Document ID: US20240239024A1
- Status: Published application
- Kind: A1
- Application number: 18/412,029
- Filed: 2024-01-12
- Published: 2024-07-18
- Earliest claimed: 2023-01-13
- Assignees: Sekisui Specialty Chemicals America, LLC
- Applicants: Sekisui Specialty Chemicals America, LLC
- Inventors: David B. Wurm; George Shitera; Vinh Nguyen
- Web page: https://patentgrep.com/patent/US20240239024A1

## CPC

- B29C 33/60: Releasing, lubricating or separating agents {(in general C10M)}
- B29C 33/68: Release sheets
- B29C 33/62: based on polymers or oligomers
- C10M 173/02: not containing mineral or fatty oils
- C10M 2207/022: containing at least two hydroxy groups
- C10M 2207/046: Hydroxy ethers
- C10M 2207/126: monocarboxylic
- C10M 2209/04: containing monomers having an unsaturated radical bound to an alcohol or ester thereof; bound to an aldehyde, ketonic, ether, ketal or acetal radical
- C10M 2209/043: used as base material
- C10M 2209/046: used as thickening agents
- C10M 2219/104: containing sulfur and carbon with nitrogen or oxygen in the ring
- C10M 2229/02: Unspecified siloxanes; Silicones
- C10N 2030/02: Pour-point; Viscosity index
- C10N 2030/06: Oiliness; Film-strength; Anti-wear; Resistance to extreme pressure
- C10N 2030/16: Antiseptic; {(micro)} biocidal {or bactericidal}
- C10N 2030/18: Anti-foaming property
- C10N 2030/24: {Emulsion properties}
- C10N 2040/36: Release agents {or mold release agents}
- C10N 2050/01: {Emulsions, colloids, or micelles}
- C10N 2050/02: dissolved or suspended in a carrier which subsequently evaporates to leave a lubricant coating
- C10N 2050/025: {in the form of films or sheets}
- B29C: SHAPING OR JOINING OF PLASTICS; SHAPING OF MATERIAL IN A PLASTIC STATE, NOT OTHERWISE PROVIDED FOR; AFTER-TREATMENT OF THE SHAPED PRODUCTS, e.g. REPAIRING (making preforms B29B11/00; making laminated products by combining previously unconnected layers which become one product whose layers will remain together B32B37/00 - B32B41/00)
- C10M: LUBRICATING COMPOSITIONS (well drilling compositions C09K8/02); USE OF CHEMICAL SUBSTANCES EITHER ALONE OR AS LUBRICATING INGREDIENTS IN A LUBRICATING COMPOSITION (mould release, i.e. separating, agents for metals B22C3/00, for plastics or substances in a plastic state, in general B29C33/56, for glass C03B40/02; textile lubricating compositions D06M11/00, D06M13/00, D06M15/00; immersion oils for microscopy G02B21/33)
- C10N: INDEXING SCHEME ASSOCIATED WITH SUBCLASS C10M RELATING TO LUBRICATING COMPOSITIONS

## Abstract

A homogeneous, aqueous mold release solution including: 5 to 90 wt % water; 3 to 40 wt % polyvinyl alcohol; 0.01 to 3.2 wt % surfactant; 1 to 20 wt % sugar alcohol; 0.005 to 1.05 wt % defoamer; and up to 50 ppm biocide, where a total of all components adds to 100 wt %. The mold release solutions have a viscosity in a range from 20 to 600 cps when measured at 23° C. In another aspect, embodiments disclosed herein relate to a homogeneous, aqueous mold release solution including: 5 to 85 wt % water; 10.5 to 15 wt % polyvinyl alcohol; 0.56 to 0.8 wt % surfactant; 1 to 8 wt % sugar alcohol; 0.01 to 0.3 wt % defoamer; and up to 50 ppm biocide, wherein a total of all components adds to 100 wt %. Also disclosed are films prepared from the mold release solutions, as well as methods of coating a substrate using such mold release solutions.

## Claims

### Claim 1

A homogeneous, aqueous mold release solution, comprising:
45 to 90 wt % water;
3 to 40 wt % of a polyvinyl alcohol;
0.01 to 3.2 wt % of a surfactant;
1 to 20 wt % of a sugar alcohol;
0.005 to 1.05 wt % of a defoamer; and
up to 50 ppm of a biocide,
wherein a total of all components adds to 100 wt %, and
wherein the homogeneous, aqueous mold release solution has a viscosity in a range from 20 to 600 cps when measured at 23° C.

### Claim 2 (depends on 1)

The homogeneous, aqueous mold release solution of claim 1, comprising:
75 to 85 wt % water;
10.5 to 15 wt % of a polyvinyl alcohol;
0.56 to 0.8 wt % of a surfactant;
1 to 8 wt % of a sugar alcohol;
0.01 to 0.3 wt % of a defoamer; and
up to 50 ppm of a biocide,
wherein a total of all components adds to 100 wt %, and
wherein the homogeneous, aqueous mold release solution has a viscosity in a range from 80 to 300 cps when measured at 23° C.

### Claim 3 (depends on 1)

The homogeneous, aqueous mold release solution of claim 1, wherein the polyvinyl alcohol is a polyvinyl alcohol homopolymer having:
a degree of hydrolysis in a range from 70 to 99 mole %; and
a 4% solution viscosity in the range from 2 to 72 cps as measured at 23° C.

### Claim 4 (depends on 1)

The homogeneous, aqueous mold release solution of claim 1, wherein the surfactant comprises an organically modified polysiloxane or a polyether modified polydimethyl siloxane (PDMS).

### Claim 5 (depends on 1)

The homogeneous, aqueous mold release solution of claim 1, wherein the defoamer comprises a colloidal mixture including an oxyalkylene glycol, a fatty acid, and colloidal particles.

### Claim 6 (depends on 5)

The homogeneous, aqueous mold release solution of claim 5, wherein the defoamer comprises a mixture of polydimethyl siloxane and the colloidal mixture.

### Claim 7 (depends on 1)

The homogeneous, aqueous mold release solution of claim 1, wherein the biocide comprises isothiazolinone.

### Claim 8 (depends on 1)

The homogeneous, aqueous mold release solution of claim 1, wherein the homogeneous, aqueous mold release solution is storage stable for a period of at least one year.

### Claim 9 (depends on 1)

The homogeneous, aqueous mold release solution of claim 1, wherein the homogeneous, aqueous mold release solution is cold storage stable for a period of at least six months.

### Claim 10 (depends on 1)

The homogeneous, aqueous mold release solution of claim 1, wherein the homogeneous, mold release solution has a viscosity in a range from 80 to 300 cps when measured at 23° C.

### Claim 11 (depends on 1)

The homogeneous, aqueous mold release solution of claim 1, wherein the homogeneous, aqueous mold release solution has a Warring Blender Foam Height in a range from 50 to 700 mm at time=0, from 10 to 350 mm at time=3 minutes, and from 0 to 300 mm at time=6 minutes, when tested according to ASTM Method E2407-04.

### Claim 12 (depends on 1)

The homogeneous, aqueous mold release solution of claim 1, wherein the homogeneous, aqueous mold release solution has a surface tension in a range from about 19 to about 33 dynes/cm as measured at 23° C. according to ASTM D1331-20.

### Claim 13 (depends on 1)

The homogenous, aqueous mold release solution of claim 1, wherein the homogeneous, aqueous mold release solution has a ratio of a 6 minute foam height as measured by ASTM E2407 to a surface tension as measured by ASTM D1331 that is less than or equal to 4.2 mm/(mN/m), and wherein a film formed from the homogeneous, aqueous mold release solution has a dry film strength that is greater than or equal to 5 MPa as measured according to ASTM D882-18.

### Claim 14 (depends on 1)

The homogeneous, aqueous mold release solution of claim 1, wherein the sugar alcohol is glycerin.

### Claim 15 (depends on 1)

A film prepared from the homogeneous, aqueous mold release solution of claim 1.

### Claim 16 (depends on 15)

The film of claim 15, wherein the film has a tensile strength in a range from 3.8 to 8 MPa as measured according to ASTM D882-18.

### Claim 17 (depends on 1)

A method of coating a substrate, comprising:
forming a solution coated substrate by spraying the homogeneous, aqueous mold release solution of claim 1 onto a substrate; and
drying the homogeneous, aqueous mold release solution of the solution coated substrate to form a film.

### Claim 18 (depends on 17)

The method of claim 17, wherein the homogeneous, aqueous mold release solution of the solution coated substrate is bubble-free.

### Claim 19 (depends on 17)

The method of claim 17, wherein the film is removable from the substrate as a single sheet of the film.

### Claim 20 (depends on 18)

The method of claim 18, wherein the homogeneous, aqueous mold release solution has a surface energy within 5 mN/m of a surface energy of the substrate, as measured according to ASTM D1331-20.