# US 2024/0204183 A1 · High-nickel positive electrode material and preparation method therefor, and lithium ion battery

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2024/0204183 A1
- Document ID: US20240204183A1
- Status: Published application
- Kind: A1
- Application number: 18/286,365
- Filed: 2022-11-09
- Published: 2024-06-20
- Earliest claimed: 2021-12-08
- Assignees: BTR Nano Tech Co., Ltd.
- Applicants: Btr Nano Tech Co., Ltd.
- Inventors: Weicheng Wen; Yu Zheng; Shunyi Yang; Youyuan Huang
- Web page: https://patentgrep.com/patent/US20240204183A1

## CPC

- H01M 4/525: of mixed oxides or hydroxides containing iron, cobalt or nickel for inserting or intercalating light metals, e.g. LiNiO2, LiCoO2 or LiCoOxFy
- H01M 10/0563: Liquid materials, e.g. for Li-SOCl2 cells
- C01G 53/42: containing alkali metals, e.g. LiNiO2
- C01G 53/84: Hydroxides
- H01M 4/131: Electrodes based on mixed oxides or hydroxides, or on mixtures of oxides or hydroxides, e.g. LiCoOx
- H01M 4/136: Electrodes based on inorganic compounds other than oxides or hydroxides, e.g. sulfides, selenides, tellurides, halogenides or LiCoFy
- H01M 4/36: Selection of substances as active materials, active masses, active liquids
- H01M 4/366: {as layered products}
- H01M 4/505: of mixed oxides or hydroxides containing manganese for inserting or intercalating light metals, e.g. LiMn2O4 or LiMn2OxFy
- H01M 4/5825: {Oxygenated metallic salts or polyanionic structures, e.g. borates, phosphates, silicates, olivines}
- H01M 4/62: Selection of inactive substances as ingredients for active masses, e.g. binders, fillers
- H01M 10/052: Li-accumulators
- C01P 2002/52: containing elements as dopants
- C01P 2002/54: one element only
- C01P 2002/76: by a space-group or by other symmetry indications
- C01P 2002/85: by XPS, EDX or EDAX data
- C01P 2004/03: obtained by SEM
- C01P 2004/30: extending in three dimensions
- C01P 2004/32: Spheres
- C01P 2004/45: Aggregated particles or particles with an intergrown morphology
- C01P 2004/50: Agglomerated particles
- C01P 2004/51: Particles with a specific particle size distribution
- C01P 2004/61: Micrometer sized, i.e. from 1-100 micrometer
- C01P 2004/80: Particles consisting of a mixture of two or more inorganic phases
- C01P 2004/84: one phase coated with the other
- C01P 2006/12: Surface area
- C01P 2006/40: Electric properties
- C01P 2006/80: Compositional purity
- H01M 10/0525: Rocking-chair batteries, i.e. batteries with lithium insertion or intercalation in both electrodes; Lithium-ion batteries
- H01M 2004/021: {Physical characteristics, e.g. porosity, surface area}
- H01M 2004/028: {Positive electrodes}
- H01M 2010/4292: {Aspects relating to capacity ratio of electrodes/electrolyte or anode/cathode}
- H01M 2300/002: Inorganic electrolyte
- Y02E 60/10: Energy storage using batteries
- H01M: PROCESSES OR MEANS, e.g. BATTERIES, FOR THE DIRECT CONVERSION OF CHEMICAL ENERGY INTO ELECTRICAL ENERGY
- C01G: COMPOUNDS CONTAINING METALS NOT COVERED BY SUBCLASSES C01D OR C01F (metal hydrides {monoborane, diborane or addition complexes thereof} C01B6/00; salts of oxyacids of halogens C01B11/00; peroxides, salts or peroxyacids C01B15/00; thiosulfates, dithionites, polythionates C01B17/64; compounds containing selenium, or tellurium C01B19/00; binary compounds of nitrogen with metals C01B21/06; azides C01B21/08; {compounds containing nitrogen, other non-metals and metal C01B21/082}; metal amides C01B21/092; nitrites C01B21/50; {compounds of noble gases C01B23/0005}; phosphides C01B25/08; salts of oxyacids of phosphorus C01B25/16; carbides C01B32/90; compounds containing silicon C01B33/00; compounds containing boron C01B35/00; compounds having molecular sieve properties but not having base-exchange properties C01B37/00; compounds having molecular sieve and base-exchange properties, e.g. crystalline zeolites, C01B39/00; cyanides C01C3/08; salts of cyanamide C01C3/16; thiocyanates C01C3/20)
- C01P: INDEXING SCHEME RELATING TO STRUCTURAL AND PHYSICAL ASPECTS OF SOLID INORGANIC COMPOUNDS
- Y02E: REDUCTION OF GREENHOUSE GAS [GHG] EMISSIONS, RELATED TO ENERGY GENERATION, TRANSMISSION OR DISTRIBUTION

## Abstract

The present disclosure relates to a high-nickel positive electrode material and a preparation method therefor and a lithium ion battery, wherein a general chemical formula of the high-nickel positive electrode material is represented by formula (1): LixNi1−(a+b+c+d+e+f)CoaM1bM2cM3dM4eM5fO2 (1), where 0.95≤x≤1.2, 0≤a≤0.15, 0≤b≤0.10, 0≤c≤0.05, 0≤d≤0.05, 0≤e≤0.05, 0≤f≤0.05, and 0<a+b+c+d+e+f≤0.2. There is a relatively small amount of Ni3+ and a relatively large amount of Ni2+ in the surface of the high-nickel material in the present disclosure, which can avoid oxidation of the surface of the positive electrode material during lithium deintercalation, and facilitate maintaining structural stability of the positive electrode material, thereby avoiding loss of the positive electrode active material and the electrolytic solution, and further improving the capacity of the positive electrode material, so that the high-temperature cycle performance of the high-nickel positive electrode material is obviously improved.

## Claims

### Claim 1

A high-nickel positive electrode material, wherein a general chemical formula of the high-nickel positive electrode material is represented by formula (1):
where 0.95≤x≤1.2, 0≤a≤0.15, 0≤b≤0.10, 0≤c≤0.05, 0≤d≤0.05, 0≤e≤0.05, 0≤f≤0.05, and 0<a+b+c+d+e+f≤0.2; and
the high-nickel positive electrode material is subjected to powder XPS measurement using AlKα rays, and after peak separation and fitting are performed on Ni2P3/2 peak appearing when a binding energy is in a range of 850 eV˜870 eV, a peak area of Ni2+ is set to be S1, a peak area of Ni3+ is set to be S2, a peak width at half height of Ni2+ is set to be α, a peak width at half height of Ni3+ is set to be β, and S1, S2, α, and β satisfy a following relationship:

### Claim 2 (depends on 1)

The positive electrode material according to claim 1, wherein the positive electrode material comprises a secondary particle and/or a primary particle, at least a part of surface of the primary particle is coated with a coating layer, and the secondary particle comprises a plurality of primary particles with the coating layer.

### Claim 3 (depends on 2)

The positive electrode material according to claim 2, wherein the coating layer comprises at least one of following features (1)˜(11):
(1) the coating layer comprises a first coating layer and a second coating layer, the first coating layer is formed on the surface of the primary particle, and the second coating layer is formed on a surface of the first coating layer;
(2) the coating layer comprises a first coating layer, and the first coating layer is formed on the surface of the primary particle;
(3) the coating layer comprises a second coating layer, and the second coating layer is formed on the surface of the primary particle;
(4) the coating layer comprises a first coating layer and a second coating layer, and the first coating layer comprises an element with a valence greater than or equal to positive trivalence in the high-nickel positive electrode material;
(5) the coating layer comprises a first coating layer and a second coating layer, and the first coating layer comprises at least one of Al, Ti, P, Si, Nb, Y, W, Cr, Zr, and La;
(6) the coating layer comprises a first coating layer and a second coating layer, and the first coating layer comprises a compound containing at least one of Al, Ti, P, Si, Nb, Y, W, Cr, Zr, and La;
(7) the coating layer comprises a first coating layer and a second coating layer, the first coating layer comprises a compound containing at least one of Al, Ti, P, Si, Nb, Y, W, Cr, Zr, and La, and the compound is at least one of oxide, hydroxide, or salt;
(8) the coating layer comprises a first coating layer and a second coating layer, and the second coating layer comprises a compound containing at least one of B, La, and Al;
(9) the coating layer comprises a first coating layer and a second coating layer, the second coating layer comprises a compound containing at least one of B, La, and Al, and the compound is at least one of oxide, acid, and lithium-containing salt;
(10) the coating layer comprises a first coating layer and a second coating layer, the second coating layer comprises a boron-containing compound, and the boron-containing compound comprises at least one of boron-containing oxide, boron-containing acid, and salt containing boron and lithium; and
(11) the coating layer comprises a first coating layer and a second coating layer, the second coating layer comprises a boron-containing compound, and the boron-containing compound comprises at least one of B2O3, H3BO3, Li2O—B2O3, Li3BO3, Li2B4O7, Li2B2O7, and Li2B8O13.

### Claim 4 (depends on 1)

The positive electrode material according to claim 1, wherein the material comprises at least one of following features (1)˜(18):
(1) the M1 comprises Mn and/or Al;
(2) the M2 comprises an element with a valence greater than or equal to positive tetravalence in the high-nickel positive electrode material;
(3) the M3 comprises an element with a valence equal to positive bivalence in the high-nickel positive electrode material;
(4) the M2 and the M3 each comprise at least one of Zr, Ti, Nb, Ce, Hf, W, Mo, Ta, Ge, Sn, Sr, Mg, and Ba, and M2 and M3 are different;
(5) the M4 comprises an element with a valence greater than or equal to positive trivalence in the high-nickel positive electrode material;
(6) the M4 comprises at least one of Al, Ti, P, Si, Nb, Y, W, Cr, Zr, and La;
(7) the M5 comprises at least one of B, La, and Al;
(8) the high-nickel positive electrode material is subjected to the powder XPS measurement using the AlKα rays: after the peak separation and the fitting are performed on the Ni2P3/2 peak appearing when the binding energy is in the range of 850 eV˜870 eV, an area ratio of Ni2+/Ni3+ is greater than 1;
(9) the high-nickel positive electrode material is subjected to the powder XPS measurement using the AlKα rays: after the peak separation and the fitting are performed on an O1S peak appearing when a binding energy is in a range of 526 eV˜540 eV, an area ratio of O1Slattice oxygen/O1Simpurity oxygen is greater than ½;
(10) a mass content of LiOH in the high-nickel positive electrode material is less than 0.3 wt %;
(11) a mass content of Li2CO3 in the high-nickel positive electrode material is less than 0.3 wt %;
(12) a crystal structure of the high-nickel positive electrode material belongs to a hexagonal crystal structure or a monoclinic crystal structure;
(13) a crystal particle morphology of the high-nickel positive electrode material comprises at least one of an approximate spherical shape, an approximate cubic shape, and an approximate rectangular parallelepiped shape;
(14) pH of the high-nickel positive electrode material is: 10<pH<12;
(15) pH of the high-nickel positive electrode material is: 10.5<pH<11.7;
(16) a powder conductivity of the high-nickel positive electrode material is greater than 0.02 S/cm;
(17) a specific surface area of the high-nickel positive electrode material is 0.3 m2/g˜0.8 m2/g; and
(18) an average particle size of the high-nickel positive electrode material is 2.5 μm˜4.5 μm.

### Claim 5

A preparation method for a high-nickel positive electrode material, comprising steps of:
mixing a metal composite hydroxide precursor, a lithium-containing compound, and a dopant, and then performing a primary heat treatment to obtain a matrix material, wherein
the dopant comprises a compound containing an element M2 and a compound containing an element M3, the compound containing the element M2 is at least one of an oxide, a hydroxide, and a lithium metal oxide containing the M2, and a valence of the M2 in the compound is greater than or equal to positive tetravalence, the compound containing the element M3 is at least one of an oxide and a hydroxide containing the M3, and a valence of the M3 in the compound is positive bivalence; and
coating the matrix material to obtain the high-nickel positive electrode material.

### Claim 6 (depends on 5)

The preparation method according to claim 5, wherein the method comprises at least one of following features (1)˜(12):
(1) a mass ratio of the metal composite hydroxide precursor, the lithium-containing compound, and the dopant is 1:(0.46˜0.49):(0.001˜0.005);
(2) a mass ratio of the metal composite hydroxide precursor, the lithium-containing compound, and the dopant is 1:(0.46˜0.48):(0.001˜0.003);
(3) an atomic ratio of total metal Me in the metal composite hydroxide precursor to Li in the lithium-containing compound is 1.0<Li/Me<1.2;
(4) the lithium-containing compound comprises a lithium-containing salt and a lithium-containing hydroxide;
(5) the lithium-containing compound comprises at least one of lithium carbonate, lithium hydroxide, lithium nitrate, and lithium acetate;
(6) the element M2 and the element M3 each comprise at least one of Zr, Ti, Nb, Ce, Hf, W, Mo, Ta, Ge, Sn, Sr, Mg, and Ba, and the M2 and the M3 are different;
(7) a molar ratio nM2:nM3 of the M2 to the M3 in the dopant is greater than or equal to 2:1;
(8) an average particle size of the dopant is 10 nm˜50 nm;
(9) a temperature of the primary heat treatment is 680° C.˜900° C.;
(10) a time of the primary heat treatment is 5 h˜20 h;
(11) a heating rate of the primary heat treatment is 50° C./h˜550° C./h; and
(12) an oxygen content of the matrix material is greater than or equal to 85%.

### Claim 7 (depends on 5)

The preparation method according to claim 5, wherein the method comprises a step of mixing the matrix material and a first coating agent, and then performing a secondary heat treatment to obtain a primary coating resultant, and the method comprises at least one of following features (1)˜(12):
(1) a mass ratio of the matrix material to the first coating agent is 1000:(0.5˜3);
(2) the first coating agent comprises a metal element or a non-metal element with a valence greater than or equal to positive trivalence;
(3) the first coating agent comprises at least one of an oxide, a salt, or a hydroxide of a metal element or a non-metal element with a valence greater than or equal to positive trivalence;
(4) the first coating agent comprises a metal element or a non-metal element with a valence greater than or equal to positive trivalence, and the metal element or the non metal element comprises at least one of Al, Ti, P, Si, Nb, Y, W, Cr, Zr, or La;
(5) the first coating agent comprises at least one of lithium aluminate, lithium titanate, lithium lanthanum titanate, yttrium oxide, aluminum oxide, and titanium oxide;
(6) an average particle size of the first coating agent is 10 nm˜50 nm;
(7) a temperature of the secondary heat treatment is 600° C.˜800° C.;
(8) a time of the secondary heat treatment is 1 h˜20 h;
(9) a heating rate of the secondary heat treatment is 50° C./h˜550° C./h;
(10) after the secondary heat treatment, a step of washing under a constant-temperature condition, and performing a drying treatment under a vacuum condition after the washing is further comprised, and a temperature of the constant-temperature condition is 10° C.˜25° C.;
(11) after the secondary heat treatment, a step of washing under a constant-temperature condition, and performing a drying treatment under a vacuum condition after the washing is further comprised, and a temperature of the drying treatment is 100° C.˜200° C.; and
(12) an oxygen content of the primary coating resultant is greater than or equal to 85%.

### Claim 8 (depends on 7)

The preparation method according to claim 7, wherein the method further comprises a step of mixing the primary coating resultant and a second coating agent and then performing a tertiary heat treatment, and the method comprises at least one of following features (1)˜(9):
(1) the second coating agent comprises a compound containing at least one of B, La, and Al;
(2) the second coating agent comprises a compound containing at least one of B, La, and Al, and the compound is an oxide, an acid, or a lithium-containing salt;
(3) the second coating agent comprises a boron-containing compound;
(4) the second coating agent comprises a boron-containing compound, and the boron-containing compound comprises a boron-containing oxide, a boron-containing acid, or a salt containing boron and lithium;
(5) the second coating agent comprises a boron-containing compound, and the boron-containing compound comprises at least one of B2O3, H3BO3, Li2O—B2O3, Li3BO3, Li2B4O7, Li2B2O7, and Li2B8O13;
(6) a mass ratio of the primary coating resultant to the second coating agent is 1: (0.0005-0.005);
(7) a temperature of the tertiary heat treatment is 200° C.˜600° C.;
(8) a time of the tertiary heat treatment is 1 h˜20 h; and
(9) a heating rate of the tertiary heat treatment is 50° C./h˜550° C./h.

### Claim 9 (depends on 5)

The preparation method according to claim 5, wherein the metal composite hydroxide precursor is obtained by performing a mixing treatment on a metal salt solution, a complexing agent, and a pH regulator.

### Claim 10 (depends on 9)

The preparation method according to claim 9, wherein the method comprises at least one of following features (1)˜(10):
(1) a mass ratio of the metal salt solution, the complexing agent, and the pH regulator is 1:(0.01˜0.10):(0.1˜0.8);
(2) the metal salt solution comprises at least one of a nickel salt solution, a cobalt salt solution, a manganese salt solution, and an aluminum salt solution;
(3) the complexing agent comprises at least one of ammonia, ammonium sulfate, ammonium chloride, ammonium carbonate, ammonium fluoride, hydrazine, ethylenediamine tetraacetic acid, nitrilotriacetic acid, uracil diacetic acid, and glycine;
(4) the pH regulator comprises at least one of sodium hydroxide and potassium hydroxide;
(5) pH of the mixing treatment is 9˜13;
(6) a temperature of the mixing treatment is 10° C.˜80° C.;
(7) a time of the mixing treatment is 10 h˜200 h;
(8) the mixing treatment is performed in a stirring state at a stirring rate of 800 rpm˜1200 rpm;
(9) after the mixing treatment, steps of solid-liquid separation, washing, and drying are further comprised; and
(10) an average particle size of the metal composite hydroxide precursor is 3 μm˜10 μm.

### Claim 11 (depends on 1)

A lithium ion battery, wherein the lithium ion battery comprises the high-nickel positive electrode material according to claim 1.

### Claim 12 (depends on 2)

The positive electrode material according to claim 2, wherein the material comprises at least one of following features (1)˜(18):
(1) the M1 comprises Mn and/or Al;
(2) the M2 comprises an element with a valence greater than or equal to positive tetravalence in the high-nickel positive electrode material;
(3) the M3 comprises an element with a valence equal to positive bivalence in the high-nickel positive electrode material;
(4) the M2 and the M3 each comprise at least one of Zr, Ti, Nb, Ce, Hf, W, Mo, Ta, Ge, Sn, Sr, Mg, and Ba, and M2 and M3 are different;
(5) the M4 comprises an element with a valence greater than or equal to positive trivalence in the high-nickel positive electrode material;
(6) the M4 comprises at least one of Al, Ti, P, Si, Nb, Y, W, Cr, Zr, and La;
(7) the M5 comprises at least one of B, La, and A;
(8) the high-nickel positive electrode material is subjected to the powder XPS measurement using the AlKα rays: after the peak separation and the fitting are performed on the Ni2P3/2 peak appearing when the binding energy is in the range of 850 eV˜870 eV, an area ratio of Ni2+/Ni3+ is greater than 1;
(9) the high-nickel positive electrode material is subjected to the powder XPS measurement using the AlKα rays: after the peak separation and the fitting are performed on an O1S peak appearing when a binding energy is in a range of 526 eV˜540 eV, an area ratio of O1Slattice oxygen/O1Simpurity oxygen is greater than ½;
(10) a mass content of LiOH in the high-nickel positive electrode material is less than 0.3 wt %;
(11) a mass content of Li2CO3 in the high-nickel positive electrode material is less than 0.3 wt %;
(12) a crystal structure of the high-nickel positive electrode material belongs to a hexagonal crystal structure or a monoclinic crystal structure;
(13) a crystal particle morphology of the high-nickel positive electrode material comprises at least one of an approximate spherical shape, an approximate cubic shape, and an approximate rectangular parallelepiped shape;
(14) pH of the high-nickel positive electrode material is: 10<pH<12;
(15) pH of the high-nickel positive electrode material is: 10.5<pH<11.7;
(16) a powder conductivity of the high-nickel positive electrode material is greater than 0.02 S/cm;
(17) a specific surface area of the high-nickel positive electrode material is 0.3 m2/g˜0.8 m2/g; and
(18) an average particle size of the high-nickel positive electrode material is 2.5 μm˜4.5 μm.

### Claim 13 (depends on 3)

The positive electrode material according to claim 3, wherein the material comprises at least one of following features (1)˜(18):
(1) the M1 comprises Mn and/or Al;
(2) the M2 comprises an element with a valence greater than or equal to positive tetravalence in the high-nickel positive electrode material;
(3) the M3 comprises an element with a valence equal to positive bivalence in the high-nickel positive electrode material;
(4) the M2 and the M3 each comprise at least one of Zr, Ti, Nb, Ce, Hf, W, Mo, Ta, Ge, Sn, Sr, Mg, and Ba, and M2 and M3 are different;
(5) the M4 comprises an element with a valence greater than or equal to positive trivalence in the high-nickel positive electrode material;
(6) the M4 comprises at least one of Al, Ti, P, Si, Nb, Y, W, Cr, Zr, and La;
(7) the M5 comprises at least one of B, La, and A;
(8) the high-nickel positive electrode material is subjected to the powder XPS measurement using the AlKα rays: after the peak separation and the fitting are performed on the Ni2P3/2 peak appearing when the binding energy is in the range of 850 eV˜870 eV, an area ratio of Ni2+/Ni3+ is greater than 1;
(9) the high-nickel positive electrode material is subjected to the powder XPS measurement using the AlKα rays: after the peak separation and the fitting are performed on an O1S peak appearing when a binding energy is in a range of 526 eV˜540 eV, an area ratio of O1Slattice oxygen/O1Simpurity oxygen is greater than ½;
(10) a mass content of LiOH in the high-nickel positive electrode material is less than 0.3 wt %;
(11) a mass content of Li2C03 in the high-nickel positive electrode material is less than 0.3 wt %;
(12) a crystal structure of the high-nickel positive electrode material belongs to a hexagonal crystal structure or a monoclinic crystal structure;
(13) a crystal particle morphology of the high-nickel positive electrode material comprises at least one of an approximate spherical shape, an approximate cubic shape, and an approximate rectangular parallelepiped shape;
(14) pH of the high-nickel positive electrode material is: 10<pH<12;
(15) pH of the high-nickel positive electrode material is: 10.5<pH<11.7;
(16) a powder conductivity of the high-nickel positive electrode material is greater than 0.02 S/cm;
(17) a specific surface area of the high-nickel positive electrode material is 0.3 m2/g˜0.8 m2/g; and
(18) an average particle size of the high-nickel positive electrode material is 2.5 μm˜4.5 μm.

### Claim 14 (depends on 6)

The preparation method according to claim 6, wherein the method comprises a step of mixing the matrix material and a first coating agent, and then performing a secondary heat treatment to obtain a primary coating resultant, and the method comprises at least one of following features (1)˜(12):
(1) a mass ratio of the matrix material to the first coating agent is 1000:(0.5˜3);
(2) the first coating agent comprises a metal element or a non-metal element with a valence greater than or equal to positive trivalence;
(3) the first coating agent comprises at least one of an oxide, a salt, or a hydroxide of a metal element or a non-metal element with a valence greater than or equal to positive trivalence;
(4) the first coating agent comprises a metal element or a non-metal element with a valence greater than or equal to positive trivalence, and the metal element or the non metal element comprises at least one of Al, Ti, P, Si, Nb, Y, W, Cr, Zr, or La;
(5) the first coating agent comprises at least one of lithium aluminate, lithium titanate, lithium lanthanum titanate, yttrium oxide, aluminum oxide, and titanium oxide;
(6) an average particle size of the first coating agent is 10 nm˜50 nm;
(7) a temperature of the secondary heat treatment is 600° C.˜800° C.;
(8) a time of the secondary heat treatment is 1 h˜20 h;
(9) a heating rate of the secondary heat treatment is 50° C./h˜550° C./h;
(10) after the secondary heat treatment, a step of washing under a constant-temperature condition, and performing a drying treatment under a vacuum condition after the washing is further comprised, and a temperature of the constant-temperature condition is 10° C.˜25° C.;
(11) after the secondary heat treatment, a step of washing under a constant-temperature condition, and performing a drying treatment under a vacuum condition after the washing is further comprised, and a temperature of the drying treatment is 100° C.˜200° C.; and
(12) an oxygen content of the primary coating resultant is greater than or equal to 85%.

### Claim 15 (depends on 6)

The preparation method according to claim 6, wherein the metal composite hydroxide precursor is obtained by performing a mixing treatment on a metal salt solution, a complexing agent, and a pH regulator.

### Claim 16 (depends on 7)

The preparation method according to claim 7, wherein the metal composite hydroxide precursor is obtained by performing a mixing treatment on a metal salt solution, a complexing agent, and a pH regulator.

### Claim 17 (depends on 8)

The preparation method according to claim 8, wherein the metal composite hydroxide precursor is obtained by performing a mixing treatment on a metal salt solution, a complexing agent, and a pH regulator.