# US 2024/0200175 A1 · Non-oriented electrical steel sheet and method for manufacturing same

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2024/0200175 A1
- Document ID: US20240200175A1
- Status: Published application
- Kind: A1
- Application number: 18/287,975
- Filed: 2022-12-19
- Published: 2024-06-20
- Earliest claimed: 2021-12-21
- Assignees: Posco
- Applicants: POSCO Co., Ltd
- Inventors: Hunju Lee; Su-Yong Shin; Yunsu Kim
- Web page: https://patentgrep.com/patent/US20240200175A1

## CPC

- C22C 38/02: containing silicon
- C21D 6/005: {containing Mn}
- C21D 6/008: {containing Si}
- C21D 8/12: during manufacturing of articles with special electromagnetic properties
- C21D 8/1222: {Hot rolling}
- C21D 8/1233: {Cold rolling}
- C21D 8/1261: {following hot rolling}
- C21D 8/1272: {Final recrystallisation annealing}
- C21D 9/46: for sheet metals
- C22C 38/00: Ferrous alloys, e.g. steel alloys (cast-iron alloys C22C37/00)
- C22C 38/001: {containing N}
- C22C 38/002: {containing In, Mg, or other elements not provided for in one single group C22C38/001 - C22C38/60}
- C22C 38/004: {Very low carbon steels, i.e. having a carbon content of less than 0,01%}
- C22C 38/008: {containing tin}
- C22C 38/04: containing manganese
- C22C 38/06: containing aluminium
- C22C 38/12: containing tungsten, tantalum, molybdenum, vanadium, or niobium
- C22C 38/14: containing titanium or zirconium
- C22C 38/18: containing chromium
- C22C 38/22: with molybdenum or tungsten
- C22C 38/24: with vanadium
- C22C 38/26: with niobium or tantalum
- C22C 38/28: with titanium or zirconium
- C22C 38/32: with boron
- C22C 38/34: with more than 1.5% by weight of silicon
- C22C 38/38: with more than 1.5% by weight of manganese
- C22C 38/60: containing lead, selenium, tellurium, or antimony, or more than 0.04% by weight of sulfur
- H01F 1/147: Alloys characterised by their composition {(treatment thereof for enhancing their electromagnetic properties C21D8/12)}
- C22C: ALLOYS (treatment of alloys C21D, C22F)
- C21D: MODIFYING THE PHYSICAL STRUCTURE OF FERROUS METALS; GENERAL DEVICES FOR HEAT TREATMENT OF FERROUS OR NON-FERROUS METALS OR ALLOYS; MAKING METAL MALLEABLE, e.g. BY DECARBURISATION OR TEMPERING (surface treatment of metallic material involving at least one process provided for in class C23 and at least one process covered by this subclass C23F17/00; unidirectional solidification of eutectic materials or unidirectional demixing of eutectoid materials C30B)
- H01F: MAGNETS; INDUCTANCES; TRANSFORMERS; SELECTION OF MATERIALS FOR THEIR MAGNETIC PROPERTIES

## Abstract

A non-oriented electrical steel sheet includes by wt %, Si: 3.0 to 4.0%, Al: 0.1 to 1.5%, Mn: 0.1 to 0.5%, Cr: 2 to 20% of Mn content, a sum of Sn and Sb: 0.006 to 0.1%, C: 0.0010 to 0.0050%, and 0.0003 to 0.0050% of at least one of N, S, Ti, Nb, and V, and balance being Fe and unavoidable impurities, in which an area fraction of a grain having a grain diameter which is 10% or less of a thickness of the steel sheet is 0.5% or more, a number fraction of the grain is 20% or more, and an average grain diameter from a central layer to a surface layer in a thickness direction of the steel sheet satisfies a relationship of D(surface)/D(center)≥0.6.

## Claims

### Claim 1

A non-oriented electrical steel sheet, comprising:
by wt %, Si: 3.0 to 4.0%, Al: 0.1 to 1.5%, Mn: 0.1 to 0.5%, Cr: 2 to 20% of Mn content, a sum of Sn and Sb: 0.006 to 0.1%, C: 0.0010 to 0.0050%, and 0.0003 to 0.0050% of at least one of N, S, Ti, Nb, and V, and balance being Fe and unavoidable impurities,
wherein an area fraction of a grain having a grain diameter which is 10% or less of a thickness of the steel sheet is 0.5% or more, a number fraction of the grain is 20% or more, and an average grain diameter from a central layer to a surface layer in a thickness direction of the steel sheet satisfies a relationship of [Equation 1] below.
D(surface)/D(center)≥0.6 [Equation 1]
(In Equation 1, D (surface): represents average grain diameter of a region from the surface layer in the thickness direction of the steel sheet to a ¼ layer, D (center): represents an average grain diameter of a region from a central layer to the ¼ layer in the thickness direction of the steel sheet.)

### Claim 2 (depends on 1)

The non-oriented electrical steel sheet of claim 1, wherein:
the average grain diameter of the steel sheet is 50 to 150 μm.

### Claim 3 (depends on 1)

The non-oriented electrical steel sheet of claim 1, wherein:
a yield strength YS (RT) of the steel sheet is 400 MPa or more and a 150° C. yield strength YS (150° C.) is 340 MPa or more.

### Claim 4 (depends on 1)

The non-oriented electrical steel sheet of claim 1, wherein:
a thickness of the steel sheet is 0.1 to 0.35 mm.

### Claim 5

A method for manufacturing non-oriented electrical steel sheet, comprising:
a step of preparing a slab containing, by wt %, Si: 3.0 to 4.0%, Al: 0.1 to 1.5%, Mn: 0.1 to 0.5%, Cr: 2 to 20% of Mn content, a sum of Sn and Sb: 0.006 to 0.1%, C: 0.0010 to 0.0050%, and 0.0003 to 0.0050% of at least one of N, S, Ti, Nb, and V, and balance being Fe and unavoidable impurities;
a step of manufacturing a hot-rolled steel sheet by heating and hot-rolling the slab;
a hot-rolled steel sheet pre-annealing step including a primary pre-annealing step of heating the hot-rolled steel sheet to 950 to 1,150° C. and then maintaining the hot-rolled steel sheet for 40 seconds or more and a secondary pre-annealing step of changing the hot-rolled steel sheet to a temperature atmosphere of 850 to 950° C. within 20 seconds and maintaining the hot-rolled steel sheet for 20 seconds or more;
a step of manufacturing a cold-rolled steel sheet by cold-rolling the hot-rolled steel sheet after the pre-annealing of the hot-rolled steel sheet; and
a final annealing step including a first final annealing step in which the cold-rolled steel sheet is heated to 900° C. or higher in a mixed atmosphere of hydrogen H2 and nitrogen N2 and then maintained for 60 seconds or less and a secondary final annealing step in which the cold-rolled steel sheet is maintained at a temperature of 650 to 850° C. for 15 seconds or more.

### Claim 6 (depends on 5)

The method of claim 5, wherein:
the slab is heated to 1,200° C. or lower.

### Claim 7 (depends on 5)

The method of claim 5, wherein:
in the step of manufacturing the hot-rolled steel sheet, finish hot rolling is performed at 800° C. or higher.

### Claim 8 (depends on 5)

The method of claim 5, wherein:
in the primary pre-annealing step, the hot-rolled steel sheet is heated at a temperature rise rate of 10° C./s or higher.

### Claim 9 (depends on 5)

The method of claim 5, wherein:
in the primary pre-annealing stop, the cold-rolled steel sheet is heated at a temperature rise rate of 25° C./s or higher.

### Claim 10 (depends on 5)

The method of claim 5, wherein:
in the final annealing step, the temperature of the cold-rolled steel sheet rises by applying a rolling direction tension of 0.75 kgf/mm2 or less.