# US 2024/0199901 A1 · Process for overspray-free application of a resin composition and resin compositions for use in the process

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2024/0199901 A1
- Document ID: US20240199901A1
- Status: Published application
- Kind: A1
- Application number: 18/287,102
- Filed: 2022-04-26
- Published: 2024-06-20
- Earliest claimed: 2021-04-28
- Assignees: Allnex Netherlands B.V.
- Applicants: Allnex Netherlands B.V.
- Inventors: Elwin Aloysius Cornelius Adrianus DE WOLF; Martin BOSMA
- Web page: https://patentgrep.com/patent/US20240199901A1

## CPC

- C09D 11/36: based on non-aqueous solvents
- B05B 13/002: {Machines or plants for applying coating liquids or other fluent materials by inkjet}
- B41M 5/0047: {by ink-jet printing}
- B41M 5/0088: {by ink-jet printing}
- C09D 5/00: Coating compositions, e.g. paints, varnishes or lacquers, characterised by their physical nature or the effects produced {(electrically insulating plastics, resins or waxes H01B3/30)}; Filling pastes
- C09D 5/04: Thixotropic paints
- C09D 7/43: Thickening agents
- C09D 7/80: Processes for incorporating ingredients
- C09D: COATING COMPOSITIONS, e.g. PAINTS, VARNISHES OR LACQUERS; FILLING PASTES; CHEMICAL PAINT OR INK REMOVERS; INKS; CORRECTING FLUIDS; WOODSTAINS; PASTES OR SOLIDS FOR COLOURING OR PRINTING; USE OF MATERIALS THEREFOR (cosmetics A61K; processes for applying liquids or other fluent materials to surfaces, in general, B05D; staining wood B27K5/02; glazes or vitreous enamels C03C; natural resins, French polish, drying-oils, driers, turpentine, per se, C09F; polishing compositions other than French polish, ski waxes C09G; adhesives or use of materials as adhesives C09J; materials for sealing or packing joints or covers C09K3/10; materials for stopping leaks C09K3/12; processes for the electrolytic or electrophoretic production of coatings C25D)
- B05B: SPRAYING APPARATUS; ATOMISING APPARATUS; NOZZLES (spray-mixers with nozzles B01F25/72; processes for applying liquids or other fluent materials to surfaces by spraying B05D)
- B41M: PRINTING, DUPLICATING, MARKING, OR COPYING PROCESSES; COLOUR PRINTING, (correction of typographical errors B41J; processes for applying transfer pictures or the like B44C1/16; fluid media for correction of typographical errors by coating C09D10/00; printing textiles D06P)

## Abstract

The invention relates to a process for overspray-free application of a non-aqueous thixotropic resin composition on a substrate surface and to non-aqueous thixotropic resin compositions for use in the process comprising a resin and a thixotropy agent comprising polyurea particles characterised in that the resin composition has a high-shear viscosity HSV measured at a shear rate of 1000±50 s−1 that is lower than 100 mPa·s and a creep compliance Jmax measured after 300 seconds using a creep stress of 1.0 Pa of lower than 250 Pa−1.

## Claims

### Claim 1

A process for overspray-free application of a resin composition on a substrate surface comprising
a. Providing a resin composition,
b. Providing an overspray-free applicator comprising a print head comprising a plate comprising a plurality of perforated holes,
c. Ejecting a plurality of droplet streams or jet streams of the resin composition from the plurality of holes on the substrate surface forming a layer of the resin composition,
wherein the resin composition is a non-aqueous thixotropic resin composition comprising a resin and a thixotropy agent comprising polyurea particles characterised in that the resin composition has
a high-shear viscosity HSV measured at 23° C. at a shear rate of 1000±50 s−1 that is lower than 100 mPa·s, preferably lower than 90 mPa·s, more preferably lower than 80 mPa·s and most preferably lower than 70 mPa·s and preferably at least 30 mPa·s, more preferably at least 40 mPa·s, even more preferably at least 50 mPa·s and
a creep compliance Jmax measured at 23° C. after 300 seconds using a creep stress of 1.0 Pa of lower than 250 Pa−1, preferably lower than 150 Pa−1 and even more preferably lower than 50 Pa−1.

### Claim 2 (depends on 1)

The process according to claim 1, wherein the amount of the polyurea particles is between 0.4 and 2.5 cwt %, preferably between 0.5 and 2.0 cwt %, more preferably between 0.6 and 1.8 cwt % or most preferably between 0.7 and 1.7 cwt %, wherein cwt % is the weight % relative to the total weight of the resin composition not including the weight of optional pigments or fillers.

### Claim 3 (depends on 1)

The process according to claim 1, wherein the print head and the substrate are at an application distance between 0.1 and 15 cm, preferably between 0.5 and 12 cm, more preferably between 1 and 10 cm, more preferably between 2 and 6 cm and preferably, the holes have a diameter between 10 and 200 micrometers, preferably between 50 and 150 micrometer, more preferably between 70 and 130 micrometer, wherein preferably the flow rate of the composition through the holes of the print head is preferably between 2 and 10 g/min per hole, preferably between 3 and 9 g/min, more preferably between 4 and 8 g/min, and the average speed of the composition exiting the hole is preferably at least 2, preferably at least 4 more preferably at least 6 and most preferably at least 8 m/s.

### Claim 4 (depends on 1)

The process according to claim 1, wherein the non-aqueous thixotropic resin composition has a Hegman fineness less than the layer thickness by at least 20%, more preferably 40% and more preferably 60%.

### Claim 5

A non-aqueous thixotropic resin composition, comprising a resin and a thixotropy agent comprising polyurea particles characterised in that the composition has
a) a high-shear viscosity HSV measured at 23° C. at a shear rate of 1000±50 s−1 that is lower than 100 mPa·s, preferably lower than 90 mPa·s, more preferably lower than 80 mPa·s and even more preferably lower than 70 mPa·s and preferably at least 30 mPa·s, more preferably at least 40 mPa·s, even more preferably at least 50 mPa·s and
b) a creep compliance Jmax measured at 23° C. after 300 seconds using a creep stress of 1.0 Pa of lower than 250 Pa−1, preferably lower than 150 Pa−1 and even more preferably lower than 50 Pa−1,
c) an amount of the polyurea particles between 0.4 and 2.5 cwt %, preferably between 0.5 and 2.0 cwt %, more preferably between 0.6 and 1.8 cwt % or most preferably between 0.7 and 1.7 cwt %,
which non-aqueous thixotropic resin composition preferably is a clear-coat composition not comprising pigments.

### Claim 6 (depends on 5)

The non-aqueous thixotropic resin composition according to claim 5, wherein the polyurea particles are the anisotropic, (semi-)crystalline particulate reaction product of a polyisocyanate, preferably a di-, or tri-isocyanate and a mono-amine or alternatively a reaction product of a polyamine, preferably a di-, or tri-amine, and a mono-isocyanate wherein preferably the polyurea particles are high efficiency polyurea particles wherein
a. the mono-amine, or in the alternative the mono-isocyanate, are at least partially chiral or
b. the polyurea particles have been formed in an acoustic vibration assisted process or
c. the polyurea particles have been formed in the presence of a resin, preferably a resin dissolved in a solvent or
d. combinations of two or more of a), b) and c), preferably a combination of a) and b) or a combination of a), b) and c).

### Claim 7 (depends on 5)

The non-aqueous thixotropic resin composition according to claim 5, wherein the polyurea particles are a reaction product of a polyisocyanate and at least one amine wherein
a. the polyisocyanate is selected from the group consisting of hexamethylene-1,6-diisocyanate (HMDI), its isocyanurate trimer or biuret, trans-cyclohexylene-1,4-diisocyanate, para- and meta-xylylene diisocyanate, toluene diisocyanate, and mixtures thereof; and/or
b. the amine is a mono-amine and is a primary amine, preferably an aliphatic amine, more preferably a (substituted) alkylamine, a branched alkylamine or a cycloalkylamine chosen from the group consisting of hexylamine, cyclohexylamine, butylamine, laurylamine, 3-methoxypropylamine, or (alkylaryl) amine chosen from the group consisting of benzylamine, R-alpha-methylbenzylamine, S-alpha-methylbenzylamine, 2-phenethylamine or mixtures thereof,
and wherein preferably the polyurea particles comprise a reaction product of benzyl amine and hexamethylene diisocyanate, of 3-Methoxypropylamine and tris-isocyanurate or more preferably of S-alpha-methylbenzylamine and hexamethylene diisocyanate.

### Claim 8 (depends on 5)

The non-aqueous thixotropic resin composition according to claim 5, wherein
a. the polyurea particles have been derived from at least partially chiral mono-amine, preferably from S-alpha-methylbenzylamine, and/or
b. the polyurea particles have been formed in an acoustic vibration assisted process, and/or
c. the polyurea particles have been formed in a solvent as a masterbatch that contains polymeric resin material in an amount lower than 40 mwt %, preferably lower than 25 mwt %, more preferably lower than 15 mwt % and most preferably lower than 10 mwt %, wherein mwt % is the weight % relative to the total weight of the masterbatch.

### Claim 9 (depends on 5)

The non-aqueous thixotropic resin composition according to claim 5, wherein the melting point (Tm1) of the polyurea particles comprised in the thixotropic resin composition is more than 10° C. below the intended curing temperature (Tcur) of the composition.

### Claim 10 (depends on 5)

The non-aqueous thixotropic resin composition according to claim 5, wherein the thixotropic resin composition comprises: (a) polyurea particles having a melting point (Tm1) at least 10° C. below the intended curing temperature (Tcur) of the composition, thereby satisfying the requirement Tm1<(Tcur−10° C.); and (b) a second thixotropy-inducing particulate component that retains its particulate nature at temperatures at least up to said curing temperature, wherein the second thixotropy-inducing particulate component (b) preferably contains polyurea particles having a melting point Tm2 of at least the curing temperature Tcur.

### Claim 11 (depends on 10)

The non-aqueous thixotropic resin composition according to claim 10, wherein the ratio of the polyurea particles (a) to the second thixotropy-inducing particulate component (b) (by weight) in the thixotropic resin composition is greater than 5:95, more preferably greater than 10:90, most preferably greater than 20:80 and lower than 95:5, more preferably lower than 90:10, most preferably lower than 80:20.

### Claim 12 (depends on 5)

The non-aqueous thixotropic resin composition according to claim 5, having a Hegman fineness value smaller than 40 micrometers, preferably smaller than 20 micrometers and even more preferably smaller than 15 micrometers.

### Claim 13 (depends on 5)

The non-aqueous thixotropic resin composition according to claim 5, which composition is a coating composition comprising a film-forming resin or an adhesive composition comprising an adhesive resin or a sealant composition comprising a sealant resin.

### Claim 14 (depends on 5)

The non-aqueous thixotropic resin composition according to claim 5, which is (I) a non-aqueous solvent-borne resin composition comprising a resin, an organic volatile solvent and substantially no water, wherein preferably the resin is a crosslinkable resin which preferably comprises a film-forming resin component and a crosslinking resin component or which is (II) a non-aqueous solvent-free resin composition comprising crosslinkable resin and substantially no organic solvent and substantially no water, wherein the crosslinkable resin preferably is a polymeric, oligomeric or monomeric resin or combinations thereof, optionally comprising reactive diluents.

### Claim 15 (depends on 5)

The non-aqueous thixotropic resin composition according to claim 5, which is a non-aqueous solvent-borne thixotropic resin composition, preferably a clear coat composition not comprising pigments, which comprises
a. a crosslinkable resin in a total amount preferably from 30 to 90, preferably from 40 to 80, more preferably from 45 to 70 cwt %, wherein preferably the crosslinkable resin comprises a film forming resin component comprising reactive functional groups A and a crosslinking resin component comprising functional groups B,
b. a volatile solvent in an amount between 10 and 70, preferably 20-60 and more preferably 30-65 cwt %
c. polyurea particles in an amount between 0.4 and 2.5 cwt %, preferably between 0.5 and 2.0 cwt %, more preferably between 0.6 and 1.8 cwt % or most preferably between 0.7 and 1.7 cwt %,
d. optional crosslinking catalyst from 0 to 10, preferably from 0.002 to 5, more preferably from 0.005 to 1 cwt %.

### Claim 16 (depends on 5)

The non-aqueous thixotropic resin composition according to claim 5 which is non-aqueous a solvent-free thixotropic resin composition comprising
a. polymeric, oligomeric and/or monomeric resin components having a actinic radiation curable functional group, preferably an ethylenically unsaturated group, more preferably (meth-)acryloyl, maleate or fumarate,
b. between 0.4 and 2.5 cwt %, preferably between 0.5 and 2.0 cwt %, more preferably between 0.6 and 1.8 cwt % or most preferably between 0.7 and 1.7 cwt % of polyurea particles,
c. optionally, from 0.001 to 10, preferably from 0.002 to 8, more preferably from 0.005 to 6 cwt % of photo-initiator.

### Claim 17 (depends on 5)

A process for the preparation of the non-aqueous thixotropic resin composition according to claim 5 comprising
a. providing a resin, polyurea particles and optionally one or more further components including crosslinking agent, organic volatile solvent, pigment, colorant, reactive diluent, curing catalyst, reactivity moderators, stabilizers and/or coating additives,
b. mixing the components in amounts to a set high-shear viscosity HSV measured at 23° C. at a shear rate of 1000±50 s−1 that is lower than 100 mPa·s, preferably lower than 90 mPa·s, preferably lower than 80 mPa·s and even more preferably lower than 70 mPa·s and preferably at least 30 mPa·s, more preferably at least 40 mPa·s, even more preferably at least 50 mPa·s and a set creep compliance Jmax measured at 23° C. after 300 seconds using a creep stress of 1.0 Pa of lower than 250 Pa−1, preferably lower than 150 Pa−1 and even more preferably lower than 50 Pa−1.

### Claim 18 (depends on 5)

Use of the non-aqueous thixotropic resin composition according to claim 5, in an overspray free application process for application of a coating resin composition, an adhesive resin composition or a sealant resin composition.

### Claim 19 (depends on 1)

A process for coating of an article, preferably an automobile part, comprising applying a coating layer of a non-aqueous thixotropic resin composition, preferably a clear-coat composition, using the overspray-free application process of claim 1 on at least part of a non-horizontal surface of the article and curing the layer to form a cured coating, wherein the non-aqueous thixotropic resin composition comprises a resin and a thixotropy agent comprising polyurea particles characterised in that the composition has
a) a high-shear viscosity HSV measured at 23° C. at a shear rate of 1000±50 s−1 that is lower than 100 mPa·s, preferably lower than 90 mPa·s, more preferably lower than 80 mPa·s and even more preferably lower than 70 mPa·s and preferably at least 30 mPa·s, more preferably at least 40 mPa·s, even more preferably at least 50 mPa·s and
b) a creep compliance Jmax measured at 23° C. after 300 seconds using a creep stress of 1.0 Pa of lower than 250 Pa−1, preferably lower than 150 Pa−1 and even more preferably lower than 50 Pa−1,
c) an amount of the polyurea particles between 0.4 and 2.5 cwt %, preferably between 0.5 and 2.0 cwt %, more preferably between 0.6 and 1.8 cwt % or most preferably between 0.7 and 1.7 cwt %,
which non-aqueous thixotropic resin composition preferably is a clear-coat composition not comprising pigments.

### Claim 20 (depends on 19)

Coated articles obtainable by the process of claim 19.