# US 2024/0199848 A1 · Polymer composition, manufacturing method of cross-linkable polymer and cross-linkable polymer

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2024/0199848 A1
- Document ID: US20240199848A1
- Status: Published application
- Kind: A1
- Application number: 18/136,986
- Filed: 2023-04-20
- Published: 2024-06-20
- Earliest claimed: 2022-12-09
- Assignees: Korea Institute of Science and Technology
- Applicants: Korea Institute of Science and Technology
- Inventors: Tae Ann KIM; Jae Hong KIM; Seungjun CHUNG; Jeong Gon SON; Jong Hyuk PARK; Sang-Soo LEE; Heesuk KIM
- Web page: https://patentgrep.com/patent/US20240199848A1

## CPC

- C08K 5/3415: Five-membered rings
- C08F 220/68: Esters
- C08J 3/24: Crosslinking, e.g. vulcanising, of macromolecules (mechanical aspects B29C35/00; crosslinking agents C08K)
- C08J 2333/14: of esters containing halogen, nitrogen, sulfur, or oxygen atoms in addition to the carboxy oxygen
- C08K: Use of inorganic or non-macromolecular organic substances as compounding ingredients (paints, inks, varnishes, dyes, polishes, adhesives C09)
- C08F: MACROMOLECULAR COMPOUNDS OBTAINED BY REACTIONS ONLY INVOLVING CARBON-TO-CARBON UNSATURATED BONDS
- C08J: WORKING-UP; GENERAL PROCESSES OF COMPOUNDING; AFTER-TREATMENT NOT COVERED BY SUBCLASSES C08B, C08C, C08F, C08G or C08H (working, e.g. shaping, of plastics B29)

## Abstract

The present invention relates to a polymer composition including a linear polymer including a stress visualization molecule positioned at a center portion of a chain and including a furan group; and a cross-linking agent that is an amine having two or more maleimide functional groups, and a cross-linkable polymer formed therefrom.

## Claims

### Claim 1

A polymer composition comprising:
a linear polymer including a stress visualization molecule positioned at a center portion of a chain and including a furan group; and
a cross-linking agent that is an amine having two or more maleimide functional groups.

### Claim 2 (depends on 1)

The polymer composition of claim 1, wherein:
the linear polymer is formed through an atom transfer radical polymerization (ARTP) reaction between the stress visualization molecule and a monomer containing a furan group.

### Claim 3 (depends on 1)

The polymer composition of claim 1, wherein:
the stress visualization molecule is substituted with an alkyl halide.

### Claim 4 (depends on 1)

The polymer composition of claim 1, wherein:
the stress visualization molecule is spiropyran, spirothiopyran, spiro rhodamine, naphthopyran, bis(adamantyl)dioxetane, or diarylbibenzofuranone substituted with an alkyl bromide.

### Claim 5 (depends on 1)

The polymer composition of claim 1, wherein:
the stress visualization molecule is represented by Chemical Formula 1:
wherein
R1 to R6 are each independently hydrogen or a substituted or unsubstituted C1-C5 alkyl group, and A1 and A2 are each independently any one of F, Cl, Br, and I.

### Claim 6 (depends on 1)

The polymer composition of claim 1, wherein:
the linear polymer is represented by Chemical Formula 2:
wherein
R7 and R8 are each independently a substituted or unsubstituted C9-C15 alkyl group,
n1 and n3 are each independently an integer of 20 to 160,
n2 and n4 are each independently an integer from 1 to 50, and
MO is the stress visualization molecule.

### Claim 7 (depends on 1)

The polymer composition of claim 1, wherein:
the cross-linking agent is represented by Chemical Formula 3:
wherein
R9 to R11 are each independently represented by hydrogen or Chemical Formula 4, where two or more of R9 to R11 are represented by Chemical Formula 4:
wherein
L1is a direct bond or a substituted or unsubstituted C1-C6 alkylene group.

### Claim 8 (depends on 1)

The polymer composition of claim 1, wherein:
a molecular weight of the linear polymer is 13,000 to 80,000 g/mol.

### Claim 9 (depends on 1)

The polymer composition of claim 1, wherein:
a ratio between the number of moles of the linear polymer and the number of moles of the cross-linking agent is 5:1 to 1:1 (linear polymer: cross-linking agent).

### Claim 10

A manufacturing method of a cross-linkable polymer, comprising:
forming a mixture by mixing a linear polymer including a stress visualization molecule positioned at a central portion of a chain and including a furan group, a cross-linking agent that is an amine having two or more maleimide functional groups, and a solvent with each other; and
forming the cross-linkable polymer by drying the mixture.

### Claim 11 (depends on 10)

The manufacturing method of a cross-linkable polymer of claim 10,
wherein:
in the forming of the mixture,
the mixing is performed at a temperature of 20 to 30° C. for 15 minutes to 3 hours.

### Claim 12 (depends on 10)

The manufacturing method of a cross-linkable polymer of claim 10, wherein:
in the forming of the cross-linkable polymer,
the drying is performed at a temperature of 30 to 70° C. for 8 to 16 hours.

### Claim 13 (depends on 10)

The manufacturing method of a cross-linkable polymer of claim 10, wherein:
in the forming of the cross-linkable polymer,
the drying is performed in a vacuum atmosphere.

### Claim 14

A cross-linkable polymer formed by cross-linking a linear polymer including a stress visualization molecule positioned at a center portion of a chain and including a furan group and a cross-linking agent that is an amine having two or more maleimide functional groups with each other.

### Claim 15 (depends on 14)

The cross-linkable polymer of claim 14, wherein:
the cross-link is formed by a Diels-Alder reaction between the furan group and the maleimide functional group.

### Claim 16 (depends on 15)

The cross-linkable polymer of claim 15, wherein:
the cross-link is reversible.

### Claim 17 (depends on 16)

The cross-linkable polymer of claim 16, wherein:
when the cross-linkable polymer is heated to a temperature of 100° C. or higher, the cross-linkable polymer is cleaved by a retro Diels-Alder reaction.

### Claim 18 (depends on 14)

The cross-linkable polymer of claim 14, wherein:
the cross-linkable polymer exhibits a purple color when stress of yield stress or more is applied to the cross-linkable polymer.

### Claim 19 (depends on 14)

The cross-linkable polymer of claim 14, wherein:
the cross-linkable polymer exhibits a purple color when it is irradiated with ultraviolet rays (UV).

### Claim 20 (depends on 14)

The cross-linkable polymer of claim 14, wherein:
the cross-linkable polymer has peaks appearing at 700±10 cm−1, 1700±10 cm−1, 1070±10 cm−1, and 1774±10 cm−1 during Fourier transform infrared spectroscopy (FT-IR) spectrum analysis.

### Claim 21 (depends on 14)

The cross-linkable polymer of claim 14, wherein:
a glass transition temperature (Tg) of the cross-linkable polymer before the cross-link is −45° C. or less.