# US 2024/0190039 A1 · Three-Dimensional (3D) Printed Mortar and Preparation Method Therefor, and 3D Printing Method for Mortar

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2024/0190039 A1
- Document ID: US20240190039A1
- Status: Published application
- Kind: A1
- Application number: 18/112,141
- Filed: 2023-02-21
- Published: 2024-06-13
- Earliest claimed: 2022-12-13
- Assignees: Hebei Quantum Intelligent Technology Co., Ltd.; Hebei Shengzhuo Building Equipment Manufacturing Co., Ltd.
- Applicants: Hebei Quantum Intelligent Technology Co., Ltd.; Hebei Shengzhuo Building Equipment Manufacturing Co., Ltd.
- Inventors: Chao ZHANG; Yi ZHAO; Gang LI; Ruihua LI; Jiawei WANG; Chenhui LI
- Web page: https://patentgrep.com/patent/US20240190039A1

## CPC

- B28B 1/001: {Rapid manufacturing of 3D objects by additive depositing, agglomerating or laminating of material (selective deposition modelling of metallic powder B22F10/00; rapid manufacturing of 3D objects in general and in particular of plastics B29C64/00)}
- B33Y 10/00: Processes of additive manufacturing
- B33Y 70/00: Materials specially adapted for additive manufacturing
- B33Y 70/10: Composites of different types of material, e.g. mixtures of ceramics and polymers or mixtures of metals and biomaterials
- C04B 7/02: Portland cement
- C04B 7/32: Aluminous cements
- C04B 14/06: Quartz; Sand
- C04B 16/02: Cellulosic materials (cellulosic waste materials, e.g. sawdust, rice husks, C04B18/24)
- C04B 16/0633: {Polypropylene}
- C04B 18/067: {Slags}
- C04B 18/08: Flue dust {, i.e. fly ash}
- C04B 22/10: containing carbon in the anion, e.g. carbonates
- C04B 24/122: {Hydroxy amines}
- C04B 24/2611: {Polyalkenes}
- C04B 24/2623: {Polyvinylalcohols; Polyvinylacetates}
- C04B 28/04: Portland cements
- C04B 28/06: Aluminous cements (monolithic refractories or refractory mortars C04B35/66)
- C04B 28/065: {Calcium aluminosulfate cements, e.g. cements hydrating into ettringite}
- C04B 40/0046: {characterised by their processing, e.g. sequence of mixing the ingredients when preparing the premixtures}
- C04B 2103/10: Accelerators; Activators
- C04B 2103/302: {Water reducers}
- C04B 2103/50: Defoamers, air detrainers
- C04B 2111/00181: {Mixtures specially adapted for three-dimensional printing (3DP), stereo-lithography or prototyping}
- Y02W 30/91: Use of waste materials as fillers for mortars or concrete
- B28B: SHAPING CLAY OR OTHER CERAMIC COMPOSITIONS; SHAPING SLAG; SHAPING MIXTURES CONTAINING CEMENTITIOUS MATERIAL, e.g. PLASTER (foundry moulding B22C; working stone or stone-like material B28D; shaping of substances in a plastic state, in general B29C; making layered products not composed wholly of these substances B32B)
- B33Y: ADDITIVE MANUFACTURING, i.e. MANUFACTURING OF THREE-DIMENSIONAL [3D] OBJECTS BY ADDITIVE DEPOSITION, ADDITIVE AGGLOMERATION OR ADDITIVE LAYERING, e.g. BY 3D PRINTING, STEREOLITHOGRAPHY OR SELECTIVE LASER SINTERING
- C04B: LIME, MAGNESIA; SLAG; CEMENTS; COMPOSITIONS THEREOF, e.g. MORTARS, CONCRETE OR LIKE BUILDING MATERIALS; ARTIFICIAL STONE {(roofing granules E04D7/005)}; CERAMICS (devitrified glass-ceramics C03C10/00); REFRACTORIES; TREATMENT OF NATURAL STONE
- Y02W: CLIMATE CHANGE MITIGATION TECHNOLOGIES RELATED TO WASTEWATER TREATMENT OR WASTE MANAGEMENT

## Abstract

The present disclosure belongs to the technical field of mortar, and in particular, to three-dimensional (3D) printed mortar and a preparation method therefor, and a 3D printing method for mortar. The mortar includes: 50-70 parts of ordinary Portland cement; 6-14 parts of sulphoaluminate cement; 2-20 parts of slag powder; 18-22 parts of fly ash; 0.25-2 parts of accelerator; 0.05-0.45 parts of cellulose ether; 0.1-0.3 parts of naphthalene series water reducer; 0.4-0.6 parts of redispersible rubber powder; 0.1-0.5 parts of defoamer; 0.1-0.5 parts of early strength agent; 0.4-1.0 part of polypropylene fiber; 100-120 parts of fine aggregate; and 30-40 parts of water. A 3D printing speed of the mortar of the present disclosure can be stably kept within 150-200 mm/s by using the above raw materials at a reasonable ratio.

## Claims

### Claim 1

Three-dimensional (3D) printed mortar, comprising the following raw materials in parts by mass:
50-70 parts of ordinary Portland cement;
6-14 parts of sulphoaluminate cement;
2-20 parts of slag powder;
18-22 parts of fly ash;
0.25-2 parts of accelerator;
0.05-0.45 parts of cellulose ether;
0.1-0.3 parts of naphthalene series water reducer;
0.4-0.6 parts of redispersible rubber powder;
0.1-0.5 parts of defoamer;
0.1-0.5 parts of early strength agent;
0.4-1.0 part of polypropylene fiber;
100-120 parts of fine aggregate; and
30-40 parts of water.

### Claim 2 (depends on 1)

The mortar according to claim 1, wherein the slag powder has a particle size of 1-75 m and a specific surface area of 420-450 m2/kg.

### Claim 3 (depends on 1)

The mortar according to claim 1, wherein the fly ash has a density of 2.2-2.3 g/cm3 and a particle size of 1-100 μm.

### Claim 4 (depends on 1)

The mortar according to claim 1, wherein the accelerator comprises a lithium carbonate accelerator.

### Claim 5 (depends on 1)

The mortar according to claim 1, wherein the early strength agent comprises a triethanolamine early strength agent.

### Claim 6 (depends on 1)

The mortar according to claim 1, wherein the redispersible rubber powder comprises vinyl acetate and ethylene copolymer rubber powder.

### Claim 7 (depends on 1)

The mortar according to claim 1, wherein the fine aggregate has a particle size of 0.35-0.5 mm and comprises quartz sand.

### Claim 8 (depends on 1)

The mortar according to claim 1, wherein the polypropylene fiber has a length of 5-7 mm and an aspect ratio of 190-210.

### Claim 9 (depends on 1)

A preparation method for the mortar according to claim 1, comprising the following steps:
conducting first mixing on the ordinary Portland cement, the sulphoaluminate cement, and the fine aggregate to obtain a first mixture;
conducting second mixing on the slag powder, the fly ash, the polypropylene fiber, the naphthalene series water reducer, the redispersible rubber powder, the cellulose ether, the defoamer, and the accelerator to obtain a second mixture;
conducting third mixing on the early strength agent and the water to obtain an early strength agent solution; and
conducting fourth mixing on the first mixture, the second mixture, and the early strength agent solution to obtain the mortar.

### Claim 10 (depends on 9)

The preparation method for the mortar according to claim 9, wherein the slag powder has a particle size of 1-75 μm and a specific surface area of 420-450 m2/kg.

### Claim 11 (depends on 9)

The preparation method for the mortar according to claim 9, wherein the fly ash has a density of 2.2-2.3 g/cm3 and a particle size of 1-100 μm.

### Claim 12 (depends on 9)

The preparation method for the mortar according to claim 9, wherein the accelerator comprises a lithium carbonate accelerator.

### Claim 13 (depends on 9)

The preparation method for the mortar according to claim 9, wherein the early strength agent comprises a triethanolamine early strength agent.

### Claim 14 (depends on 9)

The preparation method for the mortar according to claim 9, wherein the redispersible rubber powder comprises vinyl acetate and ethylene copolymer rubber powder.

### Claim 15 (depends on 9)

The preparation method for the mortar according to claim 9, wherein the fine aggregate has a particle size of 0.35-0.5 mm and comprises quartz sand.

### Claim 16 (depends on 9)

The preparation method for the mortar according to claim 9, wherein the polypropylene fiber has a length of 5-7 mm and an aspect ratio of 190-210.

### Claim 17 (depends on 1)

A 3D printing method using the mortar according to claim 1, wherein the 3D printing comprises the following step: conducting the 3D printing on the mortar at 0-35° C. and 0.1-200 mm/s; and
the mortar is the mortar according to claim 1.

### Claim 18 (depends on 17)

The 3D printing method using the mortar according to claim 17, wherein the slag powder has a particle size of 1-75 μm and a specific surface area of 420-450 m2/kg.

### Claim 19 (depends on 17)

The 3D printing method using the mortar according to claim 17, wherein the fly ash has a density of 2.2-2.3 g/cm3 and a particle size of 1-100 μm.

### Claim 20 (depends on 17)

The 3D printing method using the mortar according to claim 17, wherein the accelerator comprises a lithium carbonate accelerator.