# US 2024/0182314 A1 · Negative Electrode Material and Preparation Method thereof and Lithium Ion Battery

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2024/0182314 A1
- Document ID: US20240182314A1
- Status: Published application
- Kind: A1
- Application number: 18/284,875
- Filed: 2022-12-20
- Published: 2024-06-06
- Earliest claimed: 2021-12-29
- Assignees: Btr New Material Group Co., Ltd.; Dingyuan New Energy Technology Co., Ltd.
- Applicants: Btr New Material Group Co., Ltd.; Dingyuan New Energy Technology Co., Ltd.
- Inventors: Wei Xie; Chunlei Pang; Zhiqiang Deng; Jianguo Ren; Xueqin He
- Web page: https://patentgrep.com/patent/US20240182314A1

## CPC

- C01B 33/32: Alkali metal silicates ({C01B33/24} , C01B33/26 take precedence)
- C01B 33/325: {After-treatment, e.g. purification or stabilisation of solutions, granulation; Dissolution; Obtaining solid silicate, e.g. from a solution by spray-drying, flashing off water or adding a coagulant}
- C01B 33/113: Silicon oxides; Hydrates thereof {(preparing monoxide by reduction of siliceous material C01B33/182)}
- H01M 4/131: Electrodes based on mixed oxides or hydroxides, or on mixtures of oxides or hydroxides, e.g. LiCoOx
- H01M 4/1391: of electrodes based on mixed oxides or hydroxides, or on mixtures of oxides or hydroxides, e.g. LiCoOx
- H01M 4/364: {as mixtures}
- H01M 4/366: {as layered products}
- H01M 4/382: {Lithium (H01M4/405 takes precedence)}
- H01M 4/485: of mixed oxides or hydroxides for inserting or intercalating light metals, e.g. LiTi2O4 or LiTi2OxFy (H01M4/505, H01M4/525 take precedence)
- H01M 4/5825: {Oxygenated metallic salts or polyanionic structures, e.g. borates, phosphates, silicates, olivines}
- H01M 4/583: Carbonaceous material, e.g. graphite-intercalation compounds or CFx
- H01M 4/625: {Carbon or graphite}
- H01M 4/628: {Inhibitors, e.g. gassing inhibitors, corrosion inhibitors}
- H01M 10/0525: Rocking-chair batteries, i.e. batteries with lithium insertion or intercalation in both electrodes; Lithium-ion batteries
- C01B 32/05: Preparation or purification of carbon not covered by groups C01B32/15, C01B32/20, C01B32/25, C01B32/30
- C01P 2002/08: Intercalated structures, i.e. with atoms or molecules intercalated in their structure
- C01P 2002/72: by d-values or two theta-values, e.g. as X-ray diagram
- C01P 2002/74: by peak-intensities or a ratio thereof only
- C01P 2004/61: Micrometer sized, i.e. from 1-100 micrometer
- C01P 2004/80: Particles consisting of a mixture of two or more inorganic phases
- C01P 2004/84: one phase coated with the other
- C01P 2006/11: Powder tap density
- C01P 2006/12: Surface area
- C01P 2006/40: Electric properties
- H01M 2004/021: {Physical characteristics, e.g. porosity, surface area}
- H01M 2004/027: {Negative electrodes}
- Y02E 60/10: Energy storage using batteries
- C01B: NON-METALLIC ELEMENTS; COMPOUNDS THEREOF; {METALLOIDS OR COMPOUNDS THEREOF NOT COVERED BY SUBCLASS C01C}
- H01M: PROCESSES OR MEANS, e.g. BATTERIES, FOR THE DIRECT CONVERSION OF CHEMICAL ENERGY INTO ELECTRICAL ENERGY
- C01P: INDEXING SCHEME RELATING TO STRUCTURAL AND PHYSICAL ASPECTS OF SOLID INORGANIC COMPOUNDS
- Y02E: REDUCTION OF GREENHOUSE GAS [GHG] EMISSIONS, RELATED TO ENERGY GENERATION, TRANSMISSION OR DISTRIBUTION

## Abstract

The present disclosure relates to a negative electrode material and a preparation method thereof and a lithium ion battery, wherein the negative electrode material includes an active material, the active material includes a skeleton structure and a silicon oxygen material embedded on the skeleton structure; the skeleton structure includes a skeleton of lithium silicate located inside the active material and a skeleton of water-insoluble silicate located on a surface layer of the active material, and the skeleton of water-insoluble silicate is linked with the skeleton of lithium silicate, wherein in an XRD pattern of the negative electrode material, an intensity of a strongest diffraction characteristic peak of the lithium silicate is IA, and an intensity of a strongest diffraction characteristic peak of the water-insoluble silicate is IB, and 0.03≤IB/IA≤0.2.

## Claims

### Claim 1

A negative electrode material, wherein the negative electrode material comprises an active material, the active material comprises a skeleton structure that runs throughout the active material and a silicon oxygen material embedded on the skeleton structure, wherein the skeleton structure comprises a skeleton of lithium silicate located inside the active material and a skeleton of water-insoluble silicate located on a surface layer of the active material, and the skeleton of water-insoluble silicate is linked with the skeleton of lithium silicate, wherein
in an XRD pattern of the negative electrode material, an intensity of a strongest diffraction characteristic peak of the lithium silicate is IA, and an intensity of a strongest diffraction characteristic peak of the water-insoluble silicate is IB, and 0.03≤IB/IA≤0.2.

### Claim 2

A negative electrode material, wherein the negative electrode material comprises an active material;
the active material comprises lithium silicate, water-insoluble silicate, and a silicon oxygen material, wherein
the water-insoluble silicate is coated on a surface of the lithium silicate; and
the lithium silicate and/or the water-insoluble silicate contains the silicon oxygen material, wherein
in an XRD pattern of the negative electrode material, an intensity of a strongest diffraction characteristic peak of the lithium silicate is IA, and an intensity of a strongest diffraction characteristic peak of the water-insoluble silicate is IB, and 0.03≤IB/IA≤0.2.

### Claim 3 (depends on 1)

The negative electrode material according to claim 1, satisfying at least one of conditions a˜g below:
a. the silicon oxygen material is SiOn, where 0.5≤n≤1.5;
b. the lithium silicate comprises at least one of Li2SiO3, Li2Si2O5, Li4SiO4, Li2Si3O7, Li8SiO6, Li6Si2O7, Li4Si2O7, Li2Si4O7, and LiSiO3;
c. the water-insoluble silicate comprises zA2O·MOy·xSiO2, where M comprises at least one of Mg, Al, Ca, Ge, Cr, V, Ti, Sc, Co, Ni, Cu, Sr, Zn, Zr, Fe, and Mn, A comprises at least one of Li, Na, and K, 0.2≤x≤10.0, 1.0≤y≤3.0, and 0≤z≤5.0;
d. the water-insoluble silicate further comprises A2O·nSiO2, wherein A comprises at least one of Li, Na, and K, and 1≤n≤10;
e. a work function range of the water-insoluble silicate is 2.5 eV≤η≤7.0 eV;
f. the water-insoluble silicate is located in a depth region of 20 nm˜50 nm of a surface of the active material; and
g. a mass content of Li element in the water-insoluble silicate is W1%, and a content of Li element in the lithium silicate is W2%, and W2>W1≥0.

### Claim 4 (depends on 1)

The negative electrode material according to claim 1, satisfying at least one of conditions a˜j below:
a. the negative electrode material further comprises a carbon layer existing on a surface of the active material;
b. an average thickness of the carbon layer is 30 nm˜500 nm;
c. a tap density of the negative electrode material is 0.6 g/cm3˜1.2 g/cm3;
d. a specific surface area of the negative electrode material is 1.0 m2/g˜12.0 m2/g;
e. an average particle size of the negative electrode material is 3.0 μm˜12.0 μm;
f. a mass percentage content of carbon in the negative electrode material is 1.5 wt %˜10.0 wt %;
g. a mass percentage content of lithium in the negative electrode material is 3 wt %˜15 wt %;
h. pH of the negative electrode material is 8.5˜12.0; and
i. in the XRD pattern of the negative electrode material, the intensity of the strongest diffraction characteristic peak of the lithium silicate is IA, and the intensity of the strongest diffraction characteristic peak of the water-insoluble silicate is IB, and 0.12≤IB/IA≤0.18; and
j. a content of lithium element in the water-insoluble silicate of the negative electrode material is pm, and a total content of lithium element in the negative electrode material is pLi, where 0.01≤pm/pLi≤0.6.

### Claim 5

(canceled)

### Claim 6

(canceled)

### Claim 7

A preparation method of a negative electrode material, comprising steps of:
performing a surface etching treatment on a pre-lithiated silicon oxygen material; and
mixing the silicon oxygen material having undergone the surface etching treatment with a metal M-containing compound, and performing a solid-phase thermal reaction under a protective atmosphere, to obtain the negative electrode material.

### Claim 8 (depends on 7)

The method according to claim 7, satisfying at least one of conditions a˜d below:
a. the metal M-containing compound comprises at least one of a carbonate of metal M, an oxide of metal M, and a hydroxide of metal M, where M comprises at least one of Mg, Al, Ca, Ge, Cr, Pb, Sr, Zn, Zr, Fe, and Mn;
b. a mass ratio of the silicon oxygen material having undergone the surface etching treatment to the metal M-containing compound is 1:(0.01˜0.1);
c. a mass ratio of the silicon oxygen material having undergone the surface etching treatment to the metal M-containing compound is 1:(0.075˜0.1); and
d. the metal M-containing compound is an oxide of metal M.

### Claim 9 (depends on 7)

The method according to claim 7, satisfying at least one of conditions a˜f below:
a. the mixing comprises at least one of mechanical stirring, ultrasonic dispersion, and grinding dispersion;
b. the mixing is ball milling and mixing, and a ball milling time is 3 h˜24 h;
c. a gas of the protective atmosphere comprises at least one of nitrogen gas, helium gas, neon gas, argon gas, krypton gas, and xenon gas;
d. a temperature of the solid-phase thermal reaction is 600° C.˜1200° C.;
e. a time of the solid-phase thermal reaction is 3 h˜12; and
f. a heating rate of the solid-phase thermal reaction is 1° C./min˜5° C./min.

### Claim 10 (depends on 7)

The method according to claim 7, satisfying at least one of conditions a˜k below:
a. the pre-lithiated silicon oxygen material is a pre-lithiated carbon-coated silicon oxygen material;
b. the pre-lithiated carbon-coated silicon oxygen material is obtained by reaction of the carbon-coated silicon oxygen material with a lithium source;
c. the silicon oxygen material is SiOn, where 0.5≤n≤1.5;
d. an average particle size (D50) of the silicon oxygen material is 2.0 μm-15.0 μm;
e. a thickness of a carbon layer on a surface of the carbon-coated silicon oxygen material is 30 nm˜500 nm;
f. the lithium source comprises at least one of elemental lithium or a lithium-containing compound;
g. the lithium source comprises at least one of lithium hydride, lithium alkyl, lithium metal, lithium aluminum hydride, lithium amide, and lithium borohydride;
h. a reaction temperature of the carbon-coated silicon oxygen material and the lithium source is 150° C.˜300° C.;
i. a reaction time of the carbon-coated silicon oxygen material and the lithium source is 2.0 h˜6.0 h;
j. a mass ratio of the carbon-coated silicon oxygen material to the lithium source is 1:(0.01˜0.20); and
k. a mass percentage content of lithium in the pre-lithiated carbon-coated silicon oxygen material is 3 wt %˜20 wt %.

### Claim 11 (depends on 7)

The method according to claim 7, wherein before performing the surface etching treatment on the pre-lithiated silicon oxygen material, the method further comprises:
making the silicon oxygen material react with a lithium source to obtain the pre-lithiated silicon oxygen material; or
making a carbon-coated silicon oxygen material react with a lithium source to obtain a pre-lithiated carbon-coated silicon oxygen material.

### Claim 12 (depends on 7)

The method according to claim 7, satisfying at least one of conditions a˜c below:
a. an acid solution used in the surface etching treatment has a following characteristic: when the pre-lithiated silicon oxygen material is subjected to the surface etching treatment, pH of a reaction system for surface etching is maintained to be less than 7;
b. an acid solution used in the surface etching treatment comprises at least one of hydrochloric acid, acetic acid, nitric acid, citric acid, oxalic acid, sulfuric acid, formic acid, phenol, phosphoric acid, hydride phosphate, hydroiodic acid, hydrobromic acid, ethylene diamine tetraacetic acid, glycolic acid, gluconic acid, and succinic acid; and
c. a time of the surface etching treatment is 0.5 h˜10.0 h.

### Claim 13

(canceled)

### Claim 14 (depends on 2)

The negative electrode material according to claim 2, satisfying at least one of conditions a˜g below:
a. the silicon oxygen material is SiOn, where 0.5≤n≤1.5;
b. the lithium silicate comprises at least one of Li2SiO3, Li2Si2O5, Li4SiO4, Li2Si3O7, Li8SiO6, Li6Si2O7, Li4Si2O7, Li2Si4O7, and LiSiO3;
c. the water-insoluble silicate comprises zA2O·MOy· xSiO2, where M comprises at least one of Mg, Al, Ca, Ge, Cr, V, Ti, Sc, Co, Ni, Cu, Sr, Zn, Zr, Fe, and Mn, A comprises at least one of Li, Na, and K, 0.2≤x≤10.0, 1.0≤y≤3.0, and 0≤z≤5.0;
d. the water-insoluble silicate further comprises A2O·nSiO2, wherein A comprises at least one of Li, Na, and K, and 1≤n≤10;
e. a work function range of the water-insoluble silicate is 2.5 eV≤η≤7.0 eV;
f. the water-insoluble silicate is located in a depth region of 20 nm˜50 nm of a surface of the active material; and
g. a mass content of Li element in the water-insoluble silicate is W1%, and a content of Li element in the lithium silicate is W2%, and W2>W1≥0.

### Claim 15 (depends on 2)

The negative electrode material according to claim 2, satisfying at least one of conditions a˜j below:
a. the negative electrode material further comprises a carbon layer existing on a surface of the active material;
b. an average thickness of the carbon layer is 30 nm˜500 nm;
c. a tap density of the negative electrode material is 0.6 g/cm3˜1.2 g/cm3;
d. a specific surface area of the negative electrode material is 1.0 m2/g˜12.0 m2/g;
e. an average particle size of the negative electrode material is 3.0 μm˜12.0 μm;
f. a mass percentage content of carbon in the negative electrode material is 1.5 wt %˜10.0 wt %;
g. a mass percentage content of lithium in the negative electrode material is 3 wt %˜15 wt %;
h. pH of the negative electrode material is 8.5˜12.0; and
i. in the XRD pattern of the negative electrode material, the intensity of the strongest diffraction characteristic peak of the lithium silicate is IA, and the intensity of the strongest diffraction characteristic peak of the water-insoluble silicate is IB, and 0.12≤IB/IA≤0.18; and
j. a content of lithium element in the water-insoluble silicate of the negative electrode material is pm, and a total content of lithium element in the negative electrode material is pLi, where 0.01≤pm/pLi≤0.6.

### Claim 16 (depends on 3)

The negative electrode material according to claim 3, satisfying at least one of conditions a˜j below:
a. the negative electrode material further comprises a carbon layer existing on a surface of the active material;
b. an average thickness of the carbon layer is 30 nm˜500 nm;
c. a tap density of the negative electrode material is 0.6 g/cm3˜1.2 g/cm3;
d. a specific surface area of the negative electrode material is 1.0 m2/g˜12.0 m2/g;
e. an average particle size of the negative electrode material is 3.0 μm˜12.0 μm;
f. a mass percentage content of carbon in the negative electrode material is 1.5 wt %˜10.0 wt %;
g. a mass percentage content of lithium in the negative electrode material is 3 wt %˜15 wt %;
h. pH of the negative electrode material is 8.5˜12.0; and
i. in the XRD pattern of the negative electrode material, the intensity of the strongest diffraction characteristic peak of the lithium silicate is IA, and the intensity of the strongest diffraction characteristic peak of the water-insoluble silicate is IB, and 0.12≤IB/IA≤0.18; and
j. a content of lithium element in the water-insoluble silicate of the negative electrode material is pm, and a total content of lithium element in the negative electrode material is pLi, where 0.01≤pm/pLi≤0.6.

### Claim 17 (depends on 8)

The method according to claim 8, satisfying at least one of conditions a˜f below:
a. the mixing comprises at least one of mechanical stirring, ultrasonic dispersion, and grinding dispersion;
b. the mixing is ball milling and mixing, and a ball milling time is 3 h˜24 h;
c. a gas of the protective atmosphere comprises at least one of nitrogen gas, helium gas, neon gas, argon gas, krypton gas, and xenon gas;
d. a temperature of the solid-phase thermal reaction is 600° C.˜1200° C.;
e. a time of the solid-phase thermal reaction is 3 h˜12; and
f. a heating rate of the solid-phase thermal reaction is 1° C./min˜5° C./min.

### Claim 18 (depends on 8)

The method according to claim 8, satisfying at least one of conditions a˜k below:
a. the pre-lithiated silicon oxygen material is a pre-lithiated carbon-coated silicon oxygen material;
b. the pre-lithiated carbon-coated silicon oxygen material is obtained by reaction of the carbon-coated silicon oxygen material with a lithium source;
c. the silicon oxygen material is SiOn, where 0.5≤n≤1.5;
d. an average particle size (D50) of the silicon oxygen material is 2.0 μm-15.0 μm;
e. a thickness of a carbon layer on a surface of the carbon-coated silicon oxygen material is 30 nm˜500 nm;
f. the lithium source comprises at least one of elemental lithium or a lithium-containing compound;
g. the lithium source comprises at least one of lithium hydride, lithium alkyl, lithium metal, lithium aluminum hydride, lithium amide, and lithium borohydride;
h. a reaction temperature of the carbon-coated silicon oxygen material and the lithium source is 150° C.˜300° C.;
i. a reaction time of the carbon-coated silicon oxygen material and the lithium source is 2.0 h˜6.0 h;
j. a mass ratio of the carbon-coated silicon oxygen material to the lithium source is 1:(0.01˜0.20); and
k. a mass percentage content of lithium in the pre-lithiated carbon-coated silicon oxygen material is 3 wt %˜20 wt %.

### Claim 19 (depends on 8)

The method according to claim 8, wherein before performing the surface etching treatment on the pre-lithiated silicon oxygen material, the method further comprises:
making the silicon oxygen material react with a lithium source to obtain the pre-lithiated silicon oxygen material; or
making a carbon-coated silicon oxygen material react with a lithium source to obtain a pre-lithiated carbon-coated silicon oxygen material.

### Claim 20 (depends on 8)

The method according to claim 8, satisfying at least one of conditions a˜c below:
a. an acid solution used in the surface etching treatment has a following characteristic: when the pre-lithiated silicon oxygen material is subjected to the surface etching treatment, pH of a reaction system for surface etching is maintained to be less than 7;
b. an acid solution used in the surface etching treatment comprises at least one of hydrochloric acid, acetic acid, nitric acid, citric acid, oxalic acid, sulfuric acid, formic acid, phenol, phosphoric acid, hydride phosphate, hydroiodic acid, hydrobromic acid, ethylene diamine tetraacetic acid, glycolic acid, gluconic acid, and succinic acid; and
c. a time of the surface etching treatment is 0.5 h˜10.0 h.