# US 2024/0182313 A1 · Composite anode material, method for preparing same, and lithium-ion battery

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2024/0182313 A1
- Document ID: US20240182313A1
- Status: Published application
- Kind: A1
- Application number: 18/549,336
- Filed: 2021-11-04
- Published: 2024-06-06
- Earliest claimed: 2021-03-29
- Assignees: Btr New Material Group Co., Ltd.
- Applicants: Btr New Material Group Co., Ltd.
- Inventors: Chunlei PANG; Tengyu LIANG; Jianguo REN; Xueqin HE
- Web page: https://patentgrep.com/patent/US20240182313A1

## CPC

- C01B 33/12: Silica; Hydrates thereof, e.g. lepidoic silicic acid
- C01B 33/20: Silicates (persilicates C01B15/14 {; containing aluminium C01B33/26})
- H01M 4/0428: {Chemical vapour deposition}
- H01M 4/134: Electrodes based on metals, Si or alloys
- H01M 4/1395: of electrodes based on metals, Si or alloys
- H01M 4/36: Selection of substances as active materials, active masses, active liquids
- H01M 4/364: {as mixtures}
- H01M 4/366: {as layered products}
- H01M 4/386: {Silicon or alloys based on silicon}
- H01M 4/483: {for non-aqueous cells (H01M4/485 takes precedence)}
- H01M 4/485: of mixed oxides or hydroxides for inserting or intercalating light metals, e.g. LiTi2O4 or LiTi2OxFy (H01M4/505, H01M4/525 take precedence)
- H01M 4/583: Carbonaceous material, e.g. graphite-intercalation compounds or CFx
- H01M 4/587: for inserting or intercalating light metals
- H01M 4/625: {Carbon or graphite}
- H01M 4/628: {Inhibitors, e.g. gassing inhibitors, corrosion inhibitors}
- H01M 10/0525: Rocking-chair batteries, i.e. batteries with lithium insertion or intercalation in both electrodes; Lithium-ion batteries
- C01B 32/15: Nano-sized carbon materials
- C01P 2002/82: by IR- or Raman-data
- C01P 2004/32: Spheres
- C01P 2004/61: Micrometer sized, i.e. from 1-100 micrometer
- C01P 2004/64: Nanometer sized, i.e. from 1-100 nanometer
- C01P 2004/84: one phase coated with the other
- C01P 2006/12: Surface area
- C01P 2006/40: Electric properties
- H01M 2004/021: {Physical characteristics, e.g. porosity, surface area}
- H01M 2004/027: {Negative electrodes}
- Y02E 60/10: Energy storage using batteries
- C01B: NON-METALLIC ELEMENTS; COMPOUNDS THEREOF; {METALLOIDS OR COMPOUNDS THEREOF NOT COVERED BY SUBCLASS C01C}
- H01M: PROCESSES OR MEANS, e.g. BATTERIES, FOR THE DIRECT CONVERSION OF CHEMICAL ENERGY INTO ELECTRICAL ENERGY
- C01P: INDEXING SCHEME RELATING TO STRUCTURAL AND PHYSICAL ASPECTS OF SOLID INORGANIC COMPOUNDS
- Y02E: REDUCTION OF GREENHOUSE GAS [GHG] EMISSIONS, RELATED TO ENERGY GENERATION, TRANSMISSION OR DISTRIBUTION

## Abstract

The present disclosure relates to the field of anode materials, and provides a composite anode material, a method for preparating the composite anode material, and a lithium-ion battery. The composite anode material includes a silicon oxide material and a carbon coating layer, which is located on the surface of the silicon-oxygen material. A physical adsorption-desorption isotherm of the composite anode material is of a type II or type III, and a physical adsorption-desorption isotherm of the silicon-oxygen material is of a type IV or type V. The composite anode material, the method for preparating the same, and the lithium-ion battery provided in the present disclosure can effectively improve rate performance and cycling stability of a lithium battery.

## Claims

### Claim 1

A composite anode material, comprising: a silicon-oxygen material, and a carbon coating layer on a surface of the silicon-oxygen material, wherein a physical adsorption-desorption isotherm of the composite anode material is of a type II or type III, and a physical adsorption-desorption isotherm of the silicon-oxygen material is of a type IV or type V.

### Claim 2 (depends on 1)

The composite anode material according to claim 1, wherein the composite anode material has a carbon characteristic peak D, a carbon characteristic peak G, and a silicon characteristic peak A in a Raman spectrum, a ratio ID/IG of peak intensity Ip of the carbon characteristic peak D to peak intensity IG of the carbon characteristic peak G ranges from 0.5 to 2, and a ratio of peak intensity IA of the silicon characteristic peak A to (ID+IG) ranges from 0.1 to 10.

### Claim 3 (depends on 1)

The composite anode material according to claim 1, wherein at least one of the following conditions a to f is satisfied:
a. the silicon-oxygen material comprises SiOx, where 0<x<2;
b. the silicon-oxygen material further comprises a composite material of SiOx, the composite material of SiOx comprises at least one of a SiOx composite with SiOy, a SiOx composite with SiO2, a SiOx composite with LimSiOn, a SiOx composite with NamSiOn, a SiOx composite with KmSiOn, a SiOx composite with MgmSiOn, a SiOx composite with CamSiOn, a SiOx composite with AlmSiOn, a SiOx composite with amorphous carbon, a SiOx composite with graphite, a SiOx composite with graphene, a SiOx composite with carbon nanotube, and a SiOx composite with a polymer material, where 0<y<2 and x≠y, m≥1, and n≥1;
c. a mass percentage of oxygen in the silicon-oxygen material ranges from 0.1% to 50%;
d. the silicon-oxygen material has a silicon grain size ranging from 1 nm to 100 nm;
e. the silicon-oxygen material has a specific surface area smaller than 100 m2/g; and
f. the silicon-oxygen material has a porosity φa smaller than 10%.

### Claim 4 (depends on 1)

The composite anode material according to claim 1, wherein at least one of the following conditions a to e is satisfied:
a. particles of the composite anode material are spherical or quasi-spherical, and have a Wadell's sphericity factor greater than 0.01;
b. the composite anode material has an average particle size ranging from 1.0 μm to 50 μm;
c. the composite anode material has a porosity smaller than 10%;
d. the composite anode material has a specific surface area ranging from 1 m2/g to 50 m2/g; and
e. a mass percentage of carbon in the composite anode material ranges from 0.1% to 50%.

### Claim 5

A method for preparing a composite anode material, the method comprising the following steps:
feeding a first aliphatic hydrocarbon gas in a protective atmosphere, and preheating a silicon-oxygen material and the first aliphatic hydrocarbon gas, wherein a physical adsorption-desorption isotherm of the silicon-oxygen material is of a type IV or type V; and
feeding a second aliphatic hydrocarbon gas by intermittent pulsing, and causing the second aliphatic hydrocarbon gas to undergo chemical vapor deposition on a preheated product, to obtain the composite anode material.

### Claim 6 (depends on 5)

The method according to claim 5, wherein at least one of the following conditions a to f is satisfied:
a. the silicon-oxygen material comprises SiOx, where 0<x<2;
b. the silicon-oxygen material further comprises a composite material of SiOx, the composite material of a SiOx comprises at least one of a SiOx composite with SiOy, a SiOx composite with SiO2, a SiOx composite with LimSiOn, a SiOx composite with NamSiOn, a SiOx composite with KmSiOn, a SiOx composite with MgmSiOn, a SiOx composite with CamSiOn, a SiOx composite with AlmSiOn, a SiOx composite with amorphous carbon, a SiOx composite with graphite, a SiOx composite with graphene, a SiOx composite with carbon nanotube, and a SiOx composite with a polymer material, where 0<y<2 and x≠y, m≥1, and n≥1;
c. a mass percentage of oxygen in the silicon-oxygen material ranges from 0.1% to 50%;
d. a silicon grain size in the silicon-oxygen material ranges from 1 nm to 100 nm;
e. a specific surface area of the silicon-oxygen material is smaller than 100 m2/g; and
f. a porosity φa of the silicon-oxygen material is smaller than 10%.

### Claim 7 (depends on 5)

The method according to claim 5, wherein at least one of the following conditions a to dis satisfied:
a. the protective atmosphere comprises at least one of nitrogen, helium, neon, argon, krypton, and xenon;
b. the first aliphatic hydrocarbon gas and the second aliphatic hydrocarbon gas each independently comprise at least one of acetylene, ethylene, propyne, ethane, and propylene;
c. a ratio A of a total mass of feeding of the second aliphatic hydrocarbon gas to a weight of the silicon-oxygen material satisfies the following relation: 1.5φa/(1−φa)≤A≤15φa/(1−φa), where φa denotes a porosity of the silicon-oxygen material; and
d. gas flow rates of the first aliphatic hydrocarbon gas and the second aliphatic hydrocarbon gas each independently range from 0.1 L/min to 5 L/min.

### Claim 8 (depends on 5)

The method according to claim 5, wherein at least one of the following conditions a to e is satisfied:
a. a preheating temperature ranges from 100° C. to 600° C.;
b. a preheating time ranges from 0.5 h to 24 h;
c. a reaction temperature of the chemical vapor deposition ranges from 600° C. to 1050° C.;
d. the intermittent pulsing is at an interval of 8 s to 12 s; and
e. the intermittent pulsing has a pulse duration of 8 s to 1 min.

### Claim 9 (depends on 5)

The method according to claim 5, further comprising:
cooling and sieving the composite anode material obtained by deposition so that the composite anode material has an average particle size ranging from 1.0 μm to 50 μm.

### Claim 10 (depends on 1)

A lithium-ion battery, comprising a composite anode material according to claim 1.

### Claim 11 (depends on 2)

The composite anode material according to claim 2, wherein at least one of the following conditions a to e is satisfied:
a. particles of the composite anode material are spherical or quasi-spherical, and have a Wadell's sphericity factor greater than 0.01;
b. the composite anode material has an average particle size ranging from 1.0 μm to 50 μm;
c. the composite anode material has a porosity smaller than 10%;
d. the composite anode material has a specific surface area ranging from 1 m2/g to 50 m2/g; and
e. a mass percentage of carbon in the composite anode material ranges from 0.1% to 50%.

### Claim 12 (depends on 3)

The composite anode material according to claim 3, wherein at least one of the following conditions a to e is satisfied:
a. particles of the composite anode material are spherical or quasi-spherical, and have a Wadell's sphericity factor greater than 0.01;
b. the composite anode material has an average particle size ranging from 1.0 μm to 50 μm;
c. the composite anode material has a porosity smaller than 10%;
d. the composite anode material has a specific surface area ranging from 1 m2/g to 50 m2/g; and
e. a mass percentage of carbon in the composite anode material ranges from 0.1% to 50%.

### Claim 13 (depends on 9)

The method according to claim 9, wherein at least one of the following conditions a to e is satisfied:
a. a preheating temperature ranges from 100° C. to 600° C.;
b. a preheating time ranges from 0.5 h to 24 h;
c. a reaction temperature of the chemical vapor deposition ranges from 600° C. to 1050° C.;
d. the intermittent pulsing is at an interval of 8 s to 12 s; and