# US 2024/0181555 A1 · Resistance spot welding method

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2024/0181555 A1
- Document ID: US20240181555A1
- Status: Published application
- Kind: A1
- Application number: 18/285,571
- Filed: 2022-03-07
- Published: 2024-06-06
- Earliest claimed: 2021-04-12
- Assignees: Jfe Steel Corporation
- Applicants: Jfe Steel Corporation
- Inventors: Nao KAWABE; Chikaumi SAWANISHI; Katsutoshi TAKASHIMA; Koichi TANIGUCHI; Hiroshi MATSUDA; Daiki YAMAGISHI
- Web page: https://patentgrep.com/patent/US20240181555A1

## CPC

- B23K 11/115: {by means of two electrodes placed opposite one another on both sides of the welded parts}
- B23K 11/166: {of galvanized or tinned materials}
- B23K 2101/006: {Vehicles}
- B23K 2101/18: Sheet panels
- B23K 2101/34: Coated articles {; Surface treated articles}
- B23K 2103/04: Steel {or steel} alloys
- B23K: SOLDERING OR UNSOLDERING; WELDING; CLADDING OR PLATING BY SOLDERING OR WELDING; CUTTING BY APPLYING HEAT LOCALLY, e.g. FLAME CUTTING; WORKING BY LASER BEAM

## Abstract

A resistance spot welding method for joining two or more steel sheets including at least one zinc-coated steel sheet. The method includes a first current applying step and a second current applying step. The first current applying step involves forming a nugget having a nugget diameter of 3√t or more and 4.5√t or less by setting a current value I1 (kA) and a weld time, where t is a thickness of the thinnest steel sheet among the overlapping steel sheets. The second current applying step involves growing the nugget by repeating a cooling step for maintaining a zero-current state for 10 ms or more and less than 160 ms and a current applying step for applying a current for 20 ms or more and less than 200 ms at a current value I2 (kA) greater than or equal to the current value I1 (kA).

## Claims

### Claim 1

A resistance spot welding method comprising:
applying a current to a sheet combination of two or more overlapping steel sheets including at least one zinc-coated steel sheet with the sheet combination held and pressed by a pair of welding electrodes to join the steel sheets together,
wherein the current application includes a first current applying step and a second current applying step,
the first current applying step includes forming a nugget having a nugget diameter in a range of 3√t or more and 4.5√t or less by setting a current value I1 (kA) and a weld time, where t is a thickness of a thinnest steel sheet among the overlapping steel sheets, and
the second current applying step includes growing the nugget by repeating a cooling step for maintaining a zero-current state for in a range of 10 ms or more and less than 160 ms and a current applying step for applying a current for in a range of 20 ms or more and less than 200 ms at a current value I2 (kA) greater than or equal to the current value I1 (kA).

### Claim 2 (depends on 1)

The resistance spot welding method according to claim 1, wherein a number of repetitions of the cooling step and the current applying step in the second current applying step is in a range of 2 or more and 10 or less.

### Claim 3 (depends on 1)

The resistance spot welding method according to claim 1, wherein an amount of increase in nugget diameter in the second current applying step represented by (N2−N1) is 0.1√t or more, where N1 represents a nugget diameter (mm) formed after completion of the first current applying step, and N2 represents a nugget diameter (mm) formed after completion of the first current applying step and the second current applying step.

### Claim 4 (depends on 1)

The resistance spot welding method according to claim 1, wherein the zinc-coated steel sheet is a high strength steel sheet having a Ceq of 0.20% or more and a tensile strength of 780 MPa or more, where Ceq is represented by the following formula (1):
Ceq(%)=C+Si/30+Mn/20+2P+4S (1)
where, in formula (1), each element symbol represents an amount (mass %) of the corresponding element.

### Claim 5 (depends on 2)

The resistance spot welding method according to claim 2, wherein an amount of increase in nugget diameter in the second current applying step represented by (N2−N1) is 0.1√t or more, where N1 represents a nugget diameter (mm) formed after completion of the first current applying step, and N2 represents a nugget diameter (mm) formed after completion of the first current applying step and the second current applying step.

### Claim 6 (depends on 2)

The resistance spot welding method according to claim 2, wherein the zinc-coated steel sheet is a high strength steel sheet having a Ceq of 0.20% or more and a tensile strength of 780 MPa or more, where Ceq is represented by the following formula (1):
Ceq(%)=C+Si/30+Mn/20+2P+4S (1)
where, in formula (1), each element symbol represents an amount (mass %) of the corresponding element.

### Claim 7 (depends on 3)

The resistance spot welding method according to claim 3, wherein the zinc-coated steel sheet is a high strength steel sheet having a Ceq of 0.20% or more and a tensile strength of 780 MPa or more, where Ceq is represented by the following formula (1):
Ceq(%)=C+Si/30+Mn/20+2P+4S (1)
where, in formula (1), each element symbol represents an amount (mass %) of the corresponding element.

### Claim 8 (depends on 5)

The resistance spot welding method according to claim 5, wherein the zinc-coated steel sheet is a high strength steel sheet having a Ceq of 0.20% or more and a tensile strength of 780 MPa or more, where Ceq is represented by the following formula (1):
Ceq(%)=C+Si/30+Mn/20+2P+4S (1)
where, in formula (1), each element symbol represents an amount (mass %) of the corresponding element.