# US 2024/0167126 A1 · Spheroidal Graphite Cast Iron, Method for Manufacturing Spheroidal Graphite Cast Iron, and Spheroidizing Treatment Agent

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2024/0167126 A1
- Document ID: US20240167126A1
- Status: Published application
- Kind: A1
- Application number: 18/283,570
- Filed: 2022-03-23
- Published: 2024-05-23
- Earliest claimed: 2021-03-24
- Assignees: Proterial, Ltd.
- Applicants: Hitachi Metals, Ltd.
- Inventors: Fumiya Nanjo; Ryo Goto; Atsushi Sugimoto; Lin Wang
- Web page: https://patentgrep.com/patent/US20240167126A1

## CPC

- C22C 37/04: containing spheroidal graphite
- C21C 1/10: Making spheroidal graphite cast-iron
- C22C 33/08: Making cast-iron alloys
- C22C 33/10: including procedures for adding magnesium
- C22C 37/10: containing aluminium or silicon
- C22C: ALLOYS (treatment of alloys C21D, C22F)
- C21C: PROCESSING OF PIG-IRON, e.g. REFINING, MANUFACTURE OF WROUGHT-IRON OR STEEL; TREATMENT IN MOLTEN STATE OF FERROUS ALLOYS

## Abstract

A spheroidal graphite cast iron comprising, in mass percentage: 2.8% or more and 3.3% or less of carbon; 2.5% or more and 4.0% or less of silicon; 0.32% or more and 0.40% or less of manganese; 0.020% or more and 0.030% or less of phosphorus; 0.020% or more and 0.035% or less of sulfur; 0.030% or more and 0.050% or less of magnesium; 0.010% or more and 0.050% or less in total of lanthanum and cerium; and 0.0020% or more and 0.0050% or less of calcium, with the balance being iron and inevitable impurities.

## Claims

### Claim 1

A spheroidal graphite cast iron comprising, in mass percentage:
2.8% or more and 3.3% or less of carbon;
2.5% or more and 4.0% or less of silicon;
0.32% or more and 0.40% or less of manganese;
0.020% or more and 0.030% or less of phosphorus;
0.020% or more and 0.035% or less of sulfur;
0.030% or more and 0.050% or less of magnesium;
0.010% or more and 0.050% or less in total of lanthanum and cerium; and
0.0020% or more and 0.0050% or less of calcium, with the balance being iron and inevitable impurities.

### Claim 2 (depends on 1)

The spheroidal graphite cast iron according to claim 1, wherein, when contents of magnesium, lanthanum, cerium, and calcium expressed in mass percentage are Mg, La, Ce, and Ca, respectively, a desulfurization capacity factor DS expressed by the following equation is 0.055% or more and 0.085% or less
[
Equation
⁢
1
]
DS
=
Mg
0.76
+
(
La
+
Ce
)
2.93
+
Ca
1.25
.

### Claim 3 (depends on 1)

The spheroidal graphite cast iron according to claim 1, wherein, when a sulfur content expressed in mass percentage is S, an excess magnesium content RM expressed by the following equation is 0.015% or more and 0.045% or less
[
Equation
⁢
2
]
RM
=
Mg
-
[
S
-
{
(
La
+
Ce
)
2.93
+
Ca
1.25
}
]
×
0.76
.

### Claim 4 (depends on 1)

The spheroidal graphite cast iron according to claim 1, further comprising, in mass percentage, 0.0020% or more and 0.0050% or less of aluminum.

### Claim 5

A method for manufacturing a spheroidal graphite cast iron, which comprises the processes of:
preparing a molten metal by melting raw materials;
adding a spheroidizing treatment agent to the molten metal; and
performing casting by pouring the molten metal to which the spheroidizing treatment agent is added, into a mold to produce spheroidal graphite cast iron,
the spheroidal graphite cast iron having a composition comprising, in mass percentage:
2.8% or more and 3.3% or less of carbon;
2.5% or more and 4.0% or less of silicon;
0.32% or more and 0.40% or less of manganese;
0.020% or more and 0.030% or less of phosphorus;
0.020% or more and 0.035% or less of sulfur;
0.030% or more and 0.050% or less of magnesium;
0.010% or more and 0.050% or less in total of lanthanum and cerium; and
0.0020% or more and 0.0050% or less of calcium, with the balance being iron and inevitable impurities.

### Claim 6 (depends on 5)

The method for manufacturing a spheroidal graphite cast iron according to claim 5,
wherein the spheroidizing treatment agent is filled in an iron wire, and
wherein the process of adding the spheroidizing treatment agent is performed by immersing the spheroidizing treatment agent filled in the wire, in the molten metal within a sealed space.

### Claim 7 (depends on 5)

The method for manufacturing a spheroidal graphite cast iron according to claim 5, which further comprises a process of adding an inoculant to the molten metal to which the spheroidizing treatment agent is added.

### Claim 8 (depends on 5)

The method for manufacturing a spheroidal graphite cast iron according to claim 5, which further comprises a process of performing heat treatment on the spheroidal graphite cast iron after the process of performing the casting to produce the spheroidal graphite cast iron.

### Claim 9

A spheroidizing treatment agent comprising, in mass percentage;
45% or more and 47% or less of silicon;
14% or more and 16% or less of magnesium;
4.5% or more and 8.0% or less in total of lanthanum and cerium; and
4.5% or more and 10% or less of calcium, with the balance being iron and inevitable impurities.

### Claim 10 (depends on 9)

The spheroidizing treatment agent according to claim 9, further comprising, in mass percentage, 0.30% or more and 0.80% or less of aluminum.

### Claim 11 (depends on 9)

The spheroidizing treatment agent according to claim 9, wherein the spheroidizing treatment agent is filled in an iron wire.

### Claim 12 (depends on 2)

The spheroidal graphite cast iron according to claim 2, wherein, when a sulfur content expressed in mass percentage is S, an excess magnesium content RM expressed by the following equation is 0.015% or more and 0.045% or less
[
Equation
⁢
2
]
RM
=
Mg
-
[
S
-
{
(
La
+
Ce
)
2.93
+
Ca
1.25
}
]
×
0.76
.

### Claim 13 (depends on 2)

The spheroidal graphite cast iron according to claim 2, further comprising, in mass percentage, 0.0020% or more and 0.0050% or less of aluminum.

### Claim 14 (depends on 3)

The spheroidal graphite cast iron according to claim 3, further comprising, in mass percentage, 0.0020% or more and 0.0050% or less of aluminum.

### Claim 15 (depends on 6)

The method for manufacturing a spheroidal graphite cast iron according to claim 6, which further comprises a process of adding an inoculant to the molten metal to which the spheroidizing treatment agent is added.

### Claim 16 (depends on 6)

The method for manufacturing a spheroidal graphite cast iron according to claim 6, which further comprises a process of performing heat treatment on the spheroidal graphite cast iron after the process of performing the casting to produce the spheroidal graphite cast iron.

### Claim 17 (depends on 7)

The method for manufacturing a spheroidal graphite cast iron according to claim 7, which further comprises a process of performing heat treatment on the spheroidal graphite cast iron after the process of performing the casting to produce the spheroidal graphite cast iron.

### Claim 18 (depends on 10)