# US 2024/0026601 A1 · Silver-plated conductive nylon fiber and preparation method thereof

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2024/0026601 A1
- Document ID: US20240026601A1
- Status: Published application
- Kind: A1
- Application number: 17/798,179
- Filed: 2021-06-04
- Published: 2024-01-25
- Earliest claimed: 2021-05-31
- Assignees: Soochow University
- Applicants: Soochow University
- Inventors: Tieling XING; Xin AI; Ailing XIE; Shenzhou LU; Guoqiang CHEN
- Web page: https://patentgrep.com/patent/US20240026601A1

## CPC

- D06M 11/83: with metals; with metal-generating compounds, e.g. metal carbonyls; Reduction of metal compounds on textiles
- D06M 13/175: Unsaturated ethers, e.g. vinylethers
- D06M 13/1845: {Aromatic mono- or polycarboxylic acids}
- D06M 13/207: Substituted carboxylic acids, e.g. by hydroxy or keto groups; Anhydrides, halides or salts thereof
- D06M 13/2246: {Esters of unsaturated carboxylic acids}
- D06M 13/238: Tannins, e.g. gallotannic acids
- D06M 14/16: Polyamides
- D06M 16/00: Biochemical treatment of fibres, threads, yarns, fabrics, or fibrous goods made from such materials, e.g. enzymatic
- D06M 11/55: with sulfur trioxide; with sulfuric acid or thiosulfuric acid or their salts
- D06M 2101/34: Polyamides
- D06M 2200/00: Functionality of the treatment composition and/or properties imparted to the textile material
- D06M: TREATMENT, NOT PROVIDED FOR ELSEWHERE IN CLASS D06, OF FIBRES, THREADS, YARNS, FABRICS, FEATHERS OR FIBROUS GOODS MADE FROM SUCH MATERIALS

## Abstract

The invention provides a silver-plated conductive nylon fiber and a preparation method thereof. The method includes: immersing a nylon fiber in an aqueous solution containing a polyphenolic compound at 60° C. to 70° C., adding a water-soluble oxidant into the solution, continuously reacting at 70° C. to 80° C., and obtaining a polyphenol grafted nylon fiber, where the polyphenolic compound contains a catechol group; immersing the polyphenol grafted nylon fiber into a solution containing silver ions at 15° C. to 25° C. for reaction, and raising the temperature to 70° C. to 80° C. for continuous reaction to obtain a surface-activated nylon fiber; and carrying out chemical silver plating treatment on the surface-activated nylon fiber to obtain the silver-plated conductive nylon fiber. The method does not require a heavy metal sensitizer and therefore is non-toxic and environment-friendly, and the fiber strength is maintained.

## Claims

### Claim 1

A method for preparing a silver-plated conductive nylon fiber, comprising steps of:
(1) immersing a nylon fiber in an aqueous solution containing a polyphenolic compound at 60° C. to 70° C., adding a water-soluble oxidant into the solution, continuously reacting the resultant reaction solution at 70° C. to 80° C., and obtaining a polyphenol grafted nylon fiber after the reaction is completed, wherein the polyphenolic compound contains a catechol group, and the aqueous solution of the polyphenolic compound has a concentration of 1 g/L to 5 g/L;
(2) immersing the polyphenol grafted nylon fiber obtained in the step (1) into a solution containing silver ions at 15° C. to 25° C. for reaction, and raising the temperature to 70° C. to 80° C. for continuous reaction to obtain a surface-activated nylon fiber, wherein in the solution containing silver ions, the concentration of silver ions is 1×10−5 mol/L to 3×10−5 mol/L; and
(3) carrying out chemical silver plating treatment on the surface-activated nylon fiber obtained in the step (2) to obtain the silver-plated conductive nylon fiber.

### Claim 2 (depends on 1)

The method according to claim 1, wherein before the step (1), the method further comprises step (1a): soaking the nylon fiber in sulfuric acid with a concentration of 20 mL/L to 100 mL/L at 40° C. to 60° C. for 20 to 120 min.

### Claim 3 (depends on 1)

The method according to claim 1, wherein the chemical silver plating comprises: soaking the surface-activated nylon fiber obtained in the step (2) in a silver ammonia solution added with a reducing agent at 30° C. to 50° C. for reaction for 20 to 90 min.

### Claim 4 (depends on 3)

The method according to claim 3, wherein the reducing agent is selected from the group consisting of glucose, acetaldehyde, formaldehyde or any combination thereof.

### Claim 5 (depends on 3)

The method according to claim 3, wherein the silver ammonia solution is further added with a surfactant.

### Claim 6 (depends on 5)

The method according to claim 5, wherein the surfactant comprises polyvinylpyrrolidone and/or sodium dodecyl benzene sulfonate.

### Claim 7 (depends on 5)

The method according to claim 5, wherein the surfactant has a concentration of 5 g/L to 15 g/L.

### Claim 8 (depends on 1)

The method according to claim 1, wherein in the step (1), the polyphenolic compound is selected from the group consisting of eugenol, tannic acid, ferulic acid, chlorogenic acid and any combination thereof; the water-soluble oxidant is selected from the group consisting of sodium perborate, potassium perborate, sodium persulfate and any combination thereof; and in the reaction solution, the water-soluble oxidant has a concentration of 1 g/L to 3 g/L.

### Claim 9 (depends on 1)

The method according to claim 1, wherein after the step (3), the method further comprises a step (4): washing and dehydrating the silver-plated conductive nylon fiber, and drying at 90° C. to 140° C. for 2 to 10 min.

### Claim 10 (depends on 1)

A silver-plated conductive nylon fiber prepared by the method according to claim 1.