# US 2024/0010833 A1 · Polycarbonate composition, method for the manufacture thereof, and articles formed therefrom

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2024/0010833 A1
- Document ID: US20240010833A1
- Status: Published application
- Kind: A1
- Application number: 18/037,404
- Filed: 2021-11-18
- Published: 2024-01-11
- Earliest claimed: 2020-11-17
- Applicants: Shpp Global Technologies B.V.
- Inventors: Anna SANGREGORIO; Mark Adrianus Johannes VAN DER MEE; Tony FARRELL; Peter VOLLENBERG; Rahul PATIL
- Web page: https://patentgrep.com/patent/US20240010833A1

## CPC

- C08L 69/00: Compositions of polycarbonates; Compositions of derivatives of polycarbonates
- C08K 5/521: Esters of phosphoric acids, e.g. of H3PO4
- C08K 5/5399: Phosphorus bound to nitrogen
- C08L 67/02: Polyesters derived from dicarboxylic acids and dihydroxy compounds (C08L67/06 takes precedence)
- C08L 83/10: Block- or graft-copolymers containing polysiloxane sequences (obtained by polymerising a compound having a carbon-to-carbon double bond on to a polysiloxane C08L51/08, C08L53/00)
- C08L 85/02: containing phosphorus
- C09K 21/12: containing phosphorus
- G01V 1/04: Details
- G01V 1/155: using reciprocating masses
- C08G 77/448: containing polycarbonate sequences
- C08L 2201/02: Flame or fire retardant/resistant
- C08L 2205/025: containing two or more polymers of the same hierarchy C08L, and differing only in parameters such as density, comonomer content, molecular weight, structure
- C08L 2205/03: containing three or more polymers in a blend
- C08L: COMPOSITIONS OF MACROMOLECULAR COMPOUNDS (compositions based on polymerisable monomers C08F, C08G; artificial filaments or fibres D01F; textile treating compositions D06)
- C08K: Use of inorganic or non-macromolecular organic substances as compounding ingredients (paints, inks, varnishes, dyes, polishes, adhesives C09)
- C09K: MATERIALS FOR MISCELLANEOUS APPLICATIONS, NOT PROVIDED FOR ELSEWHERE
- G01V: GEOPHYSICS; GRAVITATIONAL MEASUREMENTS; DETECTING MASSES OR OBJECTS; TAGS (means for indicating the location of accidentally buried, e.g. snow-buried, persons A63B29/02)
- C08G: MACROMOLECULAR COMPOUNDS OBTAINED OTHERWISE THAN BY REACTIONS ONLY INVOLVING UNSATURATED CARBON-TO-CARBON BONDS

## Abstract

A polycarbonate composition includes particular amounts of a bisphenol A polycarbonate homopolymer, a particular polycarbonate-siloxane copolymer, a poly(butylene terephthalate) or a poly(ethylene terephthalate), and an organophosphorus flame retardant. Methods of making the composition and articles including the composition are also described.

## Claims

### Claim 1

A polycarbonate composition comprising:
10 to less than 86 weight percent, based on the total weight of the polycarbonate composition, of a bisphenol A polycarbonate homopolymer;
a polycarbonate-siloxane copolymer having a siloxane content of 35 to 70 weight percent, based on the total weight of the polycarbonate-siloxane copolymer;
wherein the polycarbonate-siloxane copolymer is present in an amount to provide a total siloxane content of 0.5 to 20 weight percent, based on the total weight of the polycarbonate composition;
10 to 25 weight percent of a poly(butylene terephthalate), a poly(ethylene terephthalate), or a combination thereof;
greater than 4 to 10 weight percent, based on the total weight of the polycarbonate composition, of an organophosphorus flame retardant.

### Claim 2 (depends on 1)

The polycarbonate composition of claim 1, wherein a molded sample of the polycarbonate composition exhibits:
a UL-94 rating of V0 at a thickness of 1.5 millimeters or less;
a tensile elongation retention of at least 70% after exposure to DOT 4 or DOT 5.1 brake fluid for 48 hours at a temperature of 23° C. under 0% strain tested per ISO 527 at rate of 50 mm/min relative to a non-exposed sample of the same composition; and
an Izod notched impact strength of greater than 700 joules per meter at a temperature of 23° C., as determined according to ASTM D256-10; and
optionally, one or both of:
an Izod notched impact strength of greater than 400 joules per meter at a temperature of −30° C., as determined according to ASTM D256-10; and
a melt volume rate of greater than 5 cm3/10 min determined according to ISO 1133 under a load of 5 kg at 250° C.

### Claim 3 (depends on 1)

The polycarbonate composition of claim 1,
wherein the bisphenol A polycarbonate homopolymer comprises a linear bisphenol A polycarbonate homopolymer having a weight average molecular weight of 15,000 to 40,000 grams per mole, as determined by gel permeation chromatography relative to linear bisphenol A polycarbonate standards.

### Claim 4 (depends on 1)

The polycarbonate composition of claim 1, wherein the polycarbonate-siloxane copolymer comprises bisphenol A carbonate repeating units and poly(dimethyl siloxane) repeating units.

### Claim 5 (depends on 1)

The polycarbonate composition of claim 1, wherein the polycarbonate-siloxane copolymer has a weight average molecular weight of 21,000 to 50,000 g/mol, as determined by gel permeation chromatography using a crosslinked styrene-divinyl benzene column, at a sample concentration of 1 milligram per milliliter, and as calibrated with bisphenol A polycarbonate standards.

### Claim 6 (depends on 1)

The polycarbonate composition of claim 1, wherein the organophosphorus flame retardant comprises a phosphazene, a phosphate ester, an oligomeric phosphate ester, or a combination thereof.

### Claim 7 (depends on 1)

The polycarbonate composition of claim 1, wherein one or more of the bisphenol A homopolymer carbonate, the polycarbonate-siloxane copolymer, the poly(butylene terephthalate) and the poly(ethylene terephthalate) are derived from post-consumer recycled or post-industrial recycled materials or can be produced from at least one monomer derived from bio-based or plastic waste feedstock.

### Claim 8 (depends on 1)

The polycarbonate composition of claim 1, wherein the polycarbonate composition further comprises 0.1 to 10 weight percent, based on the total weight of the polycarbonate composition, of an additive composition.

### Claim 9 (depends on 1)

The polycarbonate composition of claim 1, wherein the polycarbonate composition further comprises 0.001 to 10 weight percent of an antimicrobial agent.

### Claim 10 (depends on 1)

The polycarbonate composition of claim 1, comprising
50 to 75 weight percent of the bisphenol A polycarbonate homopolymer;
5 to 20 weight percent of the polycarbonate-siloxane copolymer;
15 to 25 weight percent of the poly(butylene terephthalate); and
4.5 to 7 weight percent of the organophosphorus flame retardant.

### Claim 11 (depends on 1)

The polycarbonate composition of claim 1, comprising
50 to 75 weight percent of the bisphenol A polycarbonate homopolymer;
5 to 20 weight percent of the polycarbonate-siloxane copolymer;
15 to 25 weight percent of the poly(ethylene terephthalate); and
4.5 to 7 weight percent of the organophosphorus flame retardant.

### Claim 12 (depends on 10)

The polycarbonate composition of claim 10, wherein
the bisphenol A polycarbonate homopolymer comprises a linear bisphenol A polycarbonate homopolymer having a weight average molecular weight of 26,000 to 40,000 grams per mole, as determined by gel permeation chromatography relative to linear bisphenol A polycarbonate standards;
the polycarbonate-siloxane copolymer comprises bisphenol A carbonate repeating units and poly(dimethyl siloxane) repeating units;
the polycarbonate-siloxane copolymer has a siloxane content of 35 to 65 weight percent based on the total weight of the polycarbonate-siloxane copolymer; and
the organophosphorus flame retardant comprises a cyclic phosphazene;
wherein a molded sample of the polycarbonate composition exhibits:
a UL-94 rating of V0 at a thickness of 1.5 millimeters or less;
a tensile elongation retention of at least 70% after exposure to DOT 4 or DOT 5.1 brake fluid for 48 hours at a temperature of 23° C. under 0% strain tested per ISO 527 at rate of 50 mm/min relative to a non-exposed sample of the same composition; and
an Izod notched impact strength of greater than 700 joules per meter at a temperature of 23° C., as determined according to ASTM D256-10; and
optionally one or both of:
an Izod notched impact strength of greater than 400 joules per meter at a temperature of −30° C., as determined according to ASTM D256-10; and
a melt volume rate of greater than 5 cm3/10 min determined according to ISO 1133 under a load of 5 kg at 250° C.

### Claim 13 (depends on 10)

The polycarbonate composition of claim 10, wherein
the bisphenol A polycarbonate homopolymer comprises a linear bisphenol A polycarbonate homopolymer having a weight average molecular weight of 26,000 to 40,000 grams per mole, as determined by gel permeation chromatography relative to linear bisphenol A polycarbonate standards;
the polycarbonate-siloxane copolymer comprises bisphenol A carbonate repeating units and poly(dimethyl siloxane) repeating units;
the polycarbonate-siloxane copolymer has a siloxane content of 35 to 65 weight percent based on the total weight of the polycarbonate-siloxane copolymer; and
the organophosphorus flame retardant comprises an oligomeric phosphate ester flame retardant comprising 5 to 15 weight percent phosphorus, based on the total weight of the oligomeric phosphate ester, preferably wherein the oligomeric phosphate ester is a solid at room temperature;
wherein a molded sample of the polycarbonate composition exhibits:
a UL-94 rating of V0 at a thickness of 1.5 millimeters or less;
a tensile elongation retention of at least 70% after exposure to DOT 4 or DOT 5.1 brake fluid for 48 hours at a temperature of 23° C. under 0% strain tested per ISO 527 at rate of 50 mm/min relative to a non-exposed sample of the same composition; and
an Izod notched impact strength of greater than 700 joules per meter at a temperature of 23° C., as determined according to ASTM D256-10; and
optionally one or both of:
an Izod notched impact strength of greater than 400 joules per meter at a temperature of −30° C., as determined according to ASTM D256-10; and
a melt volume rate of greater than 5 cm3/10 min determined according to ISO 1133 under a load of 5 kg at 250° C.

### Claim 14 (depends on 1)

A method of making the polycarbonate composition of claim 1, the method comprising melt-mixing the components of the composition, and, optionally, extruding the composition.

### Claim 15 (depends on 1)

An article comprising the polycarbonate composition of claim 1.