# US 2024/0002981 A1 · Titanium alloy sheet and method for manufacturing titanium alloy sheet

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2024/0002981 A1
- Document ID: US20240002981A1
- Status: Published application
- Kind: A1
- Application number: 18/038,038
- Filed: 2021-01-28
- Published: 2024-01-04
- Earliest claimed: 2021-01-28
- Assignees: Nippon Steel Corporation
- Applicants: Nippon Steel Corporation
- Inventors: Genki TSUKAMOTO; Tomonori KUNIEDA; Yoshiki KOIKE; Toshiyuki OKUI; Hidenori TAKEBE
- Web page: https://patentgrep.com/patent/US20240002981A1

## CPC

- C22C 14/00: Alloys based on titanium
- C22F 1/183: {of titanium or alloys based thereon}
- C22C: ALLOYS (treatment of alloys C21D, C22F)
- C22F: CHANGING THE PHYSICAL STRUCTURE OF NON-FERROUS METALS AND NON-FERROUS ALLOYS (surface treatment of metallic material involving at least one process provided for in class C23 and at least one process covered by this subclass, C23F17/00)

## Abstract

A titanium alloy thin sheet contains specific chemical components, in which, when a crystal orientation of an α-phase is expressed by an Euler angle g={φ1, Φ, φ2} according to Bunge's notation method, the orientation with maximum intensity expressed by a crystal orientation distribution function f(g) calculated with Series Rank of 16 and a Gaussian half width of 5° in texture analysis using a spherical harmonics method of an electron backscatter diffraction method is in the range of φ1: 0 to 30°, ϕ: 60 to 90°, and φ2: 0 to 60°, and a degree of accumulation of the orientation with maximum intensity is 10.0 or more, a 0.2% proof stress in a sheet width direction at 25° C. is 800 MPa or more, a Young's modulus in the sheet width direction is 125 GPa or more, and an average sheet thickness is 2.5 mm or less.

## Claims

### Claim 1

A titanium alloy sheet containing, in % by mass:
Al: more than 4.0% and 6.6% or less,
Fe: 0% or more and 2.3% or less,
V: 0% or more and 4.5% or less,
Si: 0% or more and 0.60% or less,
Ni: 0% or more and less than 0.15%,
Cr: 0% or more and less than 0.25%,
Mn: 0% or more and less than 0.25%,
C: 0% or more and less than 0.080%,
N: 0% or more and 0.050% or less,
O: 0% or more and 0.40% or less, and
a remainder of Ti and impurities,
wherein, in a case in which a crystal orientation of an α-phase is expressed by an Euler angle g={φ1, Φ, φ2} according to Bunge's notation method, the orientation with maximum intensity indicated by a crystal orientation distribution function f(g) calculated with Series Rank of 16 and a Gaussian half width of 5° in texture analysis using a spherical harmonics method of an electron backscatter diffraction method is in the range of φ1: 0 to 30°, Φ: 60 to 90°, and φ2: 0 to 60°, and a degree of accumulation of the orientation with maximum intensity is 10.0 or more,
a 0.2% proof stress in a sheet width direction at 25° C. is 800 MPa or more,
a Young's modulus in the sheet width direction is 125 GPa or more, and
an average sheet thickness is 2.5 mm or less.

### Claim 2 (depends on 1)

The titanium alloy sheet according to claim 1 containing, in % by mass, either Fe: 0.5% or more and 2.3% or less or V: 2.5% or more and 4.5% or less.

### Claim 3 (depends on 2)

The titanium alloy sheet according to claim 2 containing, in % by mass, one element or two or more elements selected from the group including Ni: less than 0.15%, Cr: less than 0.25%, and Mn: less than 0.25% in place of a part of the Fe or the V.

### Claim 4 (depends on 2)

The titanium alloy sheet according to claim 2, wherein, in a case in which one element or two or more elements selected from the group including O, N, Fe, and V are contained in place of a part of the Ti, when the O content, in % by mass, is defined as [O], the N content is defined as [N], the Fe content is defined as [Fe], and the V content is defined as [V], Q expressed by the following formula (1) is 0.340 or less.
Q=[O]+(2.77×[N])+(0.1×[Fe])+(0.025×[V]) Formula (1)

### Claim 5 (depends on 1)

The titanium alloy sheet according to claim 1, wherein a half width of a diffraction peak at 2θ=53.3±1° detected by an X-ray diffraction method using CuKα as a radiation source is 0.20° or more.

### Claim 6 (depends on 1)

The titanium alloy sheet according to claim 1 including band structures having an aspect ratio of more than 3.0 and elongated in a sheet longitudinal direction,
wherein an area fraction of the band structures is 70% or more.

### Claim 7 (depends on 1)

The titanium alloy sheet according to claim 1, wherein a dimensional accuracy of a sheet thickness thereof is 5.0% or less with respect to the average sheet thickness.

### Claim 8

A method for manufacturing a titanium alloy sheet containing, in % by mass:
Al: more than 4.0% and 6.6% or less,
Fe: 0% or more and 2.3% or less,
V: 0% or more and 4.5% or less,
Si: 0% or more and 0.60% or less,
Ni: 0% or more and less than 0.15%,
Cr: 0% or more and less than 0.25%,
Mn: 0% or more and less than 0.25%,
C: 0% or more and less than 0.080%,
N: 0% or more and 0.050% or less,
O: 0% or more and 0.40% or less, and
a remainder of Ti and impurities,
wherein, in a case in which a crystal orientation of an α-phase is expressed by an Euler angle g={φ1, Φ, φ2} according to Bunge's notation method, the orientation with maximum intensity indicated by a crystal orientation distribution function f(g) calculated with Series Rank of 16 and a Gaussian half width of 5° in texture analysis using a spherical harmonics method of an electron backscatter diffraction method is in the range of φ1: 0 to 30°, Φ: 60 to 90°, and φ2: 0 to 60°, and a degree of accumulation of the orientation with maximum intensity is 10.0 or more,
a 0.2% proof stress in a sheet width direction at 25° C. is 800 MPa or more,
a Young's modulus in the sheet width direction is 125 GPa or more, and an average sheet thickness is 2.5 mm or less, the method comprising:
heating a titanium material containing, in % by mass, Al: more than 4.0% and 6.6% or less, Fe: 0% or more and 2.3% or less, V: 0% or more and 4.5% or less, Si: 0% or more and 0.60% or less, Ni: 0% or more and less than 0.15%, Cr: 0% or more and less than 0.25%, Mn: 0% or more and less than 0.25%, C: 0% or more and less than 0.08%, N: 0% or more and 0.05% or less, O: 0% or more and 0.40% or less, and a remainder of Ti and impurities;
hot rolling the titanium material in one direction after the heating; and
performing one or more cold rolling passes on the titanium material after the hot rolling in a longitudinal direction of the titanium material,
wherein, when a B transformation point is defined as Tβ (° C.), a heating temperature of the titanium material in the heating is Tβ° C. or higher and (Tβ+150)° C. or lower,
a rolling reduction in the hot rolling is 80.0% or more,
a finishing temperature in the hot rolling is (Tβ−250)° C. or higher and (Tβ−50)° C. or lower,
in the cold rolling, a rolling reduction per cold rolling pass is 40% or less, and in the case of performing a plurality of cold rolling passes, intermediate annealing treatment is included,
in annealing conditions for the intermediate annealing treatment, an annealing temperature is 500° C. or higher and 750° C. or lower, and the annealing temperature T (° C.) and a holding time t (seconds) at the annealing temperature satisfy the following formula (2).
18000≤(T+273.15)×(Log10(t)+20)<22000 Formula (2)

### Claim 9 (depends on 8)

The method for manufacturing the titanium alloy sheet according to claim 8, wherein, after the final cold rolling pass, final annealing in which the annealing temperature is 500° C. or higher and 750° C. or lower and which satisfies the above formula (2) is performed.

### Claim 10 (depends on 3)

The titanium alloy sheet according to claim 3, wherein, in a case in which one element or two or more elements selected from the group including O, N, Fe, and V are contained in place of a part of the Ti, when the O content, in % by mass, is defined as [O], the N content is defined as [N], the Fe content is defined as [Fe], and the V content is defined as [V], Q expressed by the following formula (1) is 0.340 or less.
Q=[O]+(2.77×[N])+(0.1×[Fe])+(0.025×[V]) Formula (1)