# US 2024/0002968 A1 · Ultra-high strength cold rolled steel sheet having excellent bendability, and method of manufacturing same

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2024/0002968 A1
- Document ID: US20240002968A1
- Status: Published application
- Kind: A1
- Application number: 18/038,981
- Filed: 2021-11-29
- Published: 2024-01-04
- Earliest claimed: 2020-12-03
- Assignees: Posco
- Applicants: Posco Co., Ltd
- Inventors: Jong-Pan KONG; Yeon-Sang AHN; Joo-Hyun RYU
- Web page: https://patentgrep.com/patent/US20240002968A1

## CPC

- C21D 1/19: by interrupted quenching
- C21D 9/46: for sheet metals
- C21D 1/18: Hardening (C21D1/02 takes precedence); Quenching with or without subsequent tempering (quenching devices C21D1/62)
- C21D 1/25: Hardening, combined with annealing between 300 degrees Celsius and 600 degrees Celsius, i.e. heat refining ("Vergüten")
- C21D 1/84: Controlled slow cooling (cooling-beds for metal rolling B21B43/00)
- C21D 6/002: {containing Cr (C21D6/004 takes precedence)}
- C21D 6/005: {containing Mn}
- C21D 6/008: {containing Si}
- C21D 8/02: during manufacturing of plates or strips (C21D8/12 takes precedence)
- C21D 8/021: involving particular fabrication steps or treatments of ingots or slabs
- C21D 8/0226: {Hot rolling}
- C21D 8/0236: {Cold rolling}
- C21D 8/0263: {following hot rolling}
- C21D 8/0273: {Final recrystallisation annealing}
- C21D 8/0426: {Hot rolling}
- C21D 8/0463: {following hot rolling}
- C21D 8/0473: {Final recrystallisation annealing}
- C21D 9/48: deep-drawing sheets
- C22C 38/04: containing manganese
- C22C 38/12: containing tungsten, tantalum, molybdenum, vanadium, or niobium
- C22C 38/14: containing titanium or zirconium
- C22C 38/22: with molybdenum or tungsten
- C22C 38/26: with niobium or tantalum
- C22C 38/28: with titanium or zirconium
- C22C 38/32: with boron
- C22C 38/38: with more than 1.5% by weight of manganese
- C21D 2211/008: Martensite
- C21D: MODIFYING THE PHYSICAL STRUCTURE OF FERROUS METALS; GENERAL DEVICES FOR HEAT TREATMENT OF FERROUS OR NON-FERROUS METALS OR ALLOYS; MAKING METAL MALLEABLE, e.g. BY DECARBURISATION OR TEMPERING (surface treatment of metallic material involving at least one process provided for in class C23 and at least one process covered by this subclass C23F17/00; unidirectional solidification of eutectic materials or unidirectional demixing of eutectoid materials C30B)
- C22C: ALLOYS (treatment of alloys C21D, C22F)

## Abstract

Provided are an ultra-high strength cold rolled steel sheet having excellent bendability, and a method of manufacturing the same. The steel sheet includes 0.06 to 0.17% of C, 0.1 to 0.8% of Si, 1.9 to 2.9% of Mn, 0.005 to 0.07% of Nb, 0.004 to 0.05% of Ti, 0.0004 to 0.005% of B, 0.20% or less (excluding 0%) of Cr, and 0.04 to 0.45% of Mo, with a balance of Fe and other unavoidable impurities. a microstructure of the steel sheet includes, by area: 80 to 98% of tempered martensite and a balance of fresh martensite, bainite, ferrite, and residual austenite. An average length of lath short axis of the tempered martensite is 500 nm or less.

## Claims

### Claim 1

An ultra-high strength cold rolled steel sheet having excellent bendability comprising, by weight: 0.06 to 0.17% of C, 0.1 to 0.8% of Si, 1.9 to 2.9% of Mn, 0.005 to 0.07% of Nb, 0.004 to 0.05% of Ti, 0.0004 to 0.005% of B, 0.20% or less (excluding 0%) of Cr, and 0.04 to 0.45% of Mo, with a balance of Fe and other unavoidable impurities,
wherein the steel sheet satisfies the following Relations 1 to 3,
a microstructure includes, by area: 80 to 98% of tempered martensite and a balance of fresh martensite, bainite, ferrite, and residual austenite, and
an average length of lath short axis of the tempered martensite is 500 nm or less:
0.40≤C+Mn/6+(Cr+Mo+V)/5+(Si+Ni+Cu)/15≤0.70 [Relation 1]
110≤48.8+49 log C+35.1Mn+25.9Si+76.5Cr+105.9Mo+1325Nb≤210 [Relation 2]
0.20≤Mo+200B≤0.70 [Relation 3]
wherein contents of alloy components described are based on % by weight.

### Claim 2 (depends on 1)

The ultra-high strength cold rolled steel sheet having excellent bendability of claim 1, wherein the impurities include one or more of P, S, Al, Sb, N, Mg, Sn, Sb, Zn, and Pb as a tramp element, of which the sum is 0.1% by weight or less.

### Claim 3 (depends on 1)

The ultra-high strength cold rolled steel sheet having excellent bendability of claim 1, wherein the fresh martensite is 11% or less, bainite is 3% or less, ferrite is 3% or less, and residual austenite is 3% or less.

### Claim 4 (depends on 1)

The ultra-high strength cold rolled steel sheet having excellent bendability of claim 1, wherein the cold rolled steel sheet has a yield strength (YS) of 780 to 920 MPa, a tensile strength (TS) of 980 to 1200 MPa, an elongation rate (EL) of 8% or more, a yield ratio (YS/TS) of 0.75 or more, a hole expansion ratio (HER) of 40% or more, and a bendability (YS×EL×HER) of 300 GPa %% or more, and has no crack occurrence in a 180° complete compression bending test.

### Claim 5

A method of manufacturing an ultra-high strength cold rolled steel sheet having excellent bendability, the method comprising:
heating a slab including, by weight: 0.06 to 0.17% of C, 0.1 to 0.8% of Si, 1.9 to 2.9% of Mn, 0.005 to 0.07% of Nb, 0.004 to 0.05% of Ti, 0.0004 to 0.005% of B, 0.20% or less (excluding 0%) of Cr, and 0.04 to 0.45% of Mo with a balance of Fe and other unavoidable impurities, and satisfies the following Relations 1 to 3;
finish rolling the heated slab so that a finish rolling outlet side temperature is Ar3+50° C. to Ar3+150° C., thereby obtaining a hot rolled steel sheet;
cooling the hot rolled steel sheet to Ms+50° C. to Ms+300° C. and then winding the steel sheet;
cold rolling the wound hot rolled steel sheet to obtain a cold rolled steel sheet;
continuously annealing the cold rolled steel sheet in a temperature range of 820 to 860° C.;
crack treating the continuously annealed cold rolled steel sheet for 50 to 200 seconds;
first cooling the crack treated cold rolled steel sheet down to 620 to 700° C. at a cooling rate of 1 to 10° C./s;
second cooling the first cooled cold rolled steel sheet down to 360 to 420° C. at a cooling rate of 5 to 50° C./s; and
subjecting the second cooled cold rolled steel sheet to an overaging treatment at 370 to 420° C. or the overaging treatment after reheating,
wherein in the second cooling and the overaging treatment, the following Relations 4 to 8 are satisfied:
0.40≤C+Mn/6+(Cr+Mo+V)/5+(Si+Ni+Cu)/15≤0.70 [Relation 1]
110≤48.8+49 log C+35.1Mn+25.9Si+76.5Cr+105.9Mo+1325Nb≤210 [Relation 2]
0.20≤Mo+200B≤0.70 [Relation 3]
0≤A≤50 [Relation 4]
0≤B≤40 [Relation 5]
0≤2.8A+0.5B≤100 [Relation 6]
0≤3.1A+2.3B≤200 [Relation 7]
0.25≤(3.1A+2.3B)/(2.8A+0.5B)≤3.5 [Relation 8]
wherein contents of alloy components described in Relations 1 to 3 are based on % by weight, and A is Ms—a second cooling end temperature (° C.) and B is an overaging treatment temperature—a second cooling end temperature (° C.), in Relations 4 to 8.

### Claim 6 (depends on 5)

The method of manufacturing an ultra-high strength cold rolled steel sheet having excellent bendability of claim 5, wherein the heating of a slab is performed at 1100 to 1300° C.

### Claim 7 (depends on 5)

The method of manufacturing an ultra-high strength cold rolled steel sheet having excellent bendability of claim 5, wherein the slab has a thickness of 230 to 270 mm.

### Claim 8 (depends on 5)

The method of manufacturing an ultra-high strength cold rolled steel sheet having excellent bendability of claim 5, further comprising: after the winding, cooling the wound hot rolled steel sheet to room temperature at a cooling rate of 0.1° C./s or less.

### Claim 9 (depends on 5)

The method of manufacturing an ultra-high strength cold rolled steel sheet having excellent bendability of claim 5, wherein the cold rolling is performed at a reduction rate of 40 to 70%.

### Claim 10 (depends on 5)

The method of manufacturing an ultra-high strength cold rolled steel sheet having excellent bendability of claim 5, further comprising: after the overaging treatment, roughly rolling the overaging treated cold rolled steel sheet at an elongation rate of 0.1 to 2.0%.