# US 2024/0002966 A1 · Steel for rails and a method of manufacturing of a rail thereof

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2024/0002966 A1
- Document ID: US20240002966A1
- Status: Published application
- Kind: A1
- Application number: 18/036,946
- Filed: 2020-11-17
- Published: 2024-01-04
- Earliest claimed: 2020-11-17
- Assignees: ArcelorMittal
- Applicants: ArcelorMittal
- Inventors: Diego CARRASCAL; David ALVAREZ DIEZ; José ARANCON ALVAREZ; Wilberth SOLANO ALVAREZ
- Web page: https://patentgrep.com/patent/US20240002966A1

## CPC

- C21D 9/04: for rails
- C21D 1/02: Hardening articles or materials formed by forging or rolling, with no further heating beyond that required for the formation
- C21D 1/28: Normalising
- C21D 1/84: Controlled slow cooling (cooling-beds for metal rolling B21B43/00)
- C21D 6/004: {containing Cr and Ni}
- C21D 6/005: {containing Mn}
- C21D 6/008: {containing Si}
- C21D 8/00: Modifying the physical properties of ferrous metals or ferrous alloys by deformation combined with, or followed by, heat treatment (hardening articles or materials formed by forging or rolling with no further heating beyond that required for the formation C21D1/02)
- C22C 38/001: {containing N}
- C22C 38/002: {containing In, Mg, or other elements not provided for in one single group C22C38/001 - C22C38/60}
- C22C 38/04: containing manganese
- C22C 38/06: containing aluminium
- C22C 38/20: with copper
- C22C 38/22: with molybdenum or tungsten
- C22C 38/24: with vanadium
- C22C 38/28: with titanium or zirconium
- C22C 38/34: with more than 1.5% by weight of silicon
- C22C 38/38: with more than 1.5% by weight of manganese
- C22C 38/42: with copper
- C22C 38/44: with molybdenum or tungsten
- C22C 38/46: with vanadium
- C22C 38/50: with titanium or zirconium
- C22C 38/58: with more than 1.5% by weight of manganese
- C21D 2211/005: Ferrite
- C21D 2211/009: Pearlite
- C21D: MODIFYING THE PHYSICAL STRUCTURE OF FERROUS METALS; GENERAL DEVICES FOR HEAT TREATMENT OF FERROUS OR NON-FERROUS METALS OR ALLOYS; MAKING METAL MALLEABLE, e.g. BY DECARBURISATION OR TEMPERING (surface treatment of metallic material involving at least one process provided for in class C23 and at least one process covered by this subclass C23F17/00; unidirectional solidification of eutectic materials or unidirectional demixing of eutectoid materials C30B)
- C22C: ALLOYS (treatment of alloys C21D, C22F)

## Abstract

A steel for rail having the following elements, 0.25%≤C≤0.8%; 1.0%≤Mn≤2.0%; 1.40%≤Si≤2%; 0.01%≤Al≤1%; 0.8%≤Cr≤2%; 0≤P≤0.09%; 0≤S≤0.09%; 0%≤N≤0.09%; 0%≤Ni≤1%; 0%≤Mo≤0.5%; 0%≤V≤0.2%; 0%≤Nb ≤0.1%; 0%≤Ti≤0.1%; 0%≤Cu≤0.5%; 0%≤B≤0.008%; 0%≤Sn≤0.1%; 0% ≤Ce≤0.1%; 0%≤Mg≤0.10%; 0%≤Zr≤0.10%; the remainder composition being composed of iron and unavoidable impurities caused by processing, the microstructure having, by area percentage, 2% to 10% of Proeutectoid Ferrite, the balance being made of Pearlite wherein the pearlite having interlamellar spacing from 100 nm to 250 nm .

## Claims

### Claim at position 1

1-15. (canceled)

### Claim 16

A steel for rail comprising of the following elements, expressed in percentage by weight:
0.25%≤C≤0.8%;
1.0%≤Mn≤2.0%;
1.40%≤Si≤2%;
0.01%≤Al≤1%;
0.8%≤Cr≤2%;
0≤P≤0.09%;
0≤S≤0.09%;
0%≤N≤0.09%;
and optionally including one or more of the followiing elements
0%≤Ni≤1%;
0%≤Mo≤0.5%;
0%≤V≤0.2%
0%≤Nb≤0.1%;
0%≤Ti≤0.1%;
0%≤Ce≤0.1%;
0%≤Mg≤0.10%;
0%≤Zr≤0.10%;
a remainder composition being composed of iron and unavoidable impurities caused by processing,
a microstructure of the steel comprising, by area percentage, 2% to 10% of Proeutectoid Ferrite, the balance being made of Pearlite wherein the pearlite has interlamellar spacing from 100 nm to 250 nm.

### Claim 17 (depends on 16)

The steel as recited in claim 16 wherein the composition includes 0.27% to 0.75% of Carbon.

### Claim 18 (depends on 16)

The steel as recited in claim 16 wherein the composition the composition includes 0.02% to 0.9% of Aluminum.

### Claim 19 (depends on 16)

The steel as recited in claim 16 wherein the composition the composition includes 0.9% to 1.9% of Chromium.

### Claim 20 (depends on 16)

The steel as recited in claim 16 wherein the Pearlite is between 93% and 99%.

### Claim 21 (depends on 16)

The steel as recited in claim 16 wherein the interlamellar spacing of pearlite is from 110 nm to 230 nm.

### Claim 22 (depends on 16)

The steel as recited in claim 16 wherein a tensile strength at 180° C. is greater than 900 MPa.

### Claim 23 (depends on 16)

The steel as recited in claim 16 wherein the steel has hardness of 310 Hv or more.

### Claim 24 (depends on 16)

The steel as recited in claim 16 wherein the steel has a resistivity of more than 40 Ωmm/m2.

### Claim 25 (depends on 16)

The steel as recited in claim 16 wherein the steel has a maximum permeability equal to more than 165 or more measure at 4000 A/m.

### Claim 26

A method of production of a rail of steel, the method comprising the following successive steps:
providing a steel composition in the form of semi-finished product, the steel composition expressed in percentage by weight including:
0.25%≤C≤0.8%;
1.0%≤Mn≤2.0%;
1.40%≤Si≤2%;
0.01%≤Al≤1%;
0.8%≤Cr≤2%;
0≤P≤0.09%;
0≤S≤0.09%;
0%≤N≤0.09%;
and optionally including one or more of the followiing elements
0%≤Ni≤1%;
0%≤Mo≤0.5%;
0%≤V≤0.2%
0%≤Nb≤0.1%;
0%≤Ti≤0.1%;
0%≤Cu≤0.5%;
0%≤B≤0.008%;
0%≤Sn≤0.1%;
0%≤Ce≤0.1%;
0%≤Mg≤0.10%;
0%≤Zr≤0.10%;
a remainder composition being composed of iron and unavoidable impurities caused by processing;
reheating the semi-finished product to a temperature from Ac3 to Ac3+500° C. and holding at the temperature from 5 seconds to 1200 seconds;
performing one or more hot rolling passes on the semi-finished product in the austenitic range at a hot rolling temperature from Ac3 to Ac3+300° C. to obtain a hot rail; and
cooling hot rail in two-step cooling, wherein in step one the hot rail is cooled at a cooling rate from 0.1° C./s to 5° C./s from Ac3 and Ac3+300° C. temperature to a temperature T1 ranging from 480 to 550° C., and thereafter in step two the hot rail is cooled at a cooling rate less 5° C./s from T1 to room temperature to obtain a rail.

### Claim 27 (depends on 26)

The method as recited in claim 26 wherein the reheating temperature of the semi-finished product to is from Ac3+30° C. to Ac3+450° C.

### Claim 28 (depends on 26)

The method as recited in claim 26 wherein the temperature T1 is from 490° C. to 530° C.

### Claim 29 (depends on 26)

The method as recited in claim 26 wherein the CR1 cooling rate is higher than CR2.

### Claim 30 (depends on 26)

A method for the manufacture of structural or safety parts of a rail wagon comprising the method as recited in claim 26.

### Claim 30 (depends on 16)

A method for the manufacture of structural or safety parts of a rail wagon comprising the employing the steel as recited in claim 16.