# US 2024/0002280 A1 · Enamel composition, method for preparing enamel composition, and cooking appliance

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2024/0002280 A1
- Document ID: US20240002280A1
- Status: Published application
- Kind: A1
- Application number: 18/367,628
- Filed: 2023-09-13
- Published: 2024-01-04
- Earliest claimed: 2019-02-22
- Assignees: LG Electronics Inc.
- Applicants: LG Electronics Inc.
- Inventors: Dong Gun GWOO; Jingon Kim; Young Seok Kim
- Web page: https://patentgrep.com/patent/US20240002280A1

## CPC

- C03C 3/062: with less than 40% silica by weight
- C03C 8/08: containing phosphorus
- A47J 36/025: {Vessels with non-stick features, e.g. coatings}
- A47J 36/04: the materials being non-metallic
- C03C 1/00: Ingredients generally applicable to manufacture of glasses, glazes, or vitreous enamels
- C03C 3/064: containing boron
- C03C 3/066: containing zinc
- C03C 3/068: containing rare earths
- C03C 4/20: for chemical resistant glass
- C23D 1/00: Melting or fritting the enamels; Apparatus or furnaces therefor
- C23D 5/02: by wet methods
- F24C 15/005: {Coatings for ovens}
- F24C 15/02: Doors specially adapted for stoves or ranges
- C03C 17/04: by fritting glass powder
- C03C 2207/04: for steel
- C03C 2218/17: from a solid phase
- C03C: CHEMICAL COMPOSITION OF GLASSES, GLAZES OR VITREOUS ENAMELS; SURFACE TREATMENT OF GLASS; SURFACE TREATMENT OF FIBRES OR FILAMENTS MADE FROM GLASS, MINERALS OR SLAGS; JOINING GLASS TO GLASS OR OTHER MATERIALS
- A47J: KITCHEN EQUIPMENT; COFFEE MILLS; SPICE MILLS; APPARATUS FOR MAKING BEVERAGES
- C23D: ENAMELLING OF, OR APPLYING A VITREOUS LAYER TO, METALS
- F24C: DOMESTIC STOVES OR RANGES (exclusively for solid fuels F24B); DETAILS OF DOMESTIC STOVES OR RANGES, OF GENERAL APPLICATION

## Abstract

An enamel composition, a method for preparing an enamel composition, and a cooking appliance are provided. The enamel composition may include phosphorus pentoxide (P2O5) at 15 to 50 wt %; silicon dioxide (SiO2) at 10 to 20 wt %; boron oxide (B2O3) at 1 to 15 wt %; one or more of lithium oxide (Li2O), sodium oxide (Na2O), or potassium oxide (K2O) at 5 to 20 wt %; one or more of sodium fluoride (NaF), calcium fluoride (CaF2), or aluminum fluoride (AlF3) at 1 to 5 wt %; one or more of magnesium oxide (MgO), barium oxide (BaO), or calcium oxide (CaO) at 1 to 35 wt %; and one or more of titanium dioxide (TiO2), cerium dioxide (CeO2), molybdenum trioxide (MoO3), bismuth oxide (Bi2O3), or copper oxide (CuO) at 10 to 25 wt %, such that a heating time required for cleaning may be shortened and oil contaminants may be completely removed.

## Claims

### Claim 1

A method for preparing an enamel composition, comprising:
providing materials for the enamel composition, the materials including:
phosphorus pentoxide (P2O5) at 15 to 50 wt %;
silicon dioxide (SiO2) at 10 to 20 wt %;
boron oxide (B2O3) at 1 to 15 wt %;
one or more of lithium superoxide (Li2O), sodium oxide (Na2O), or potassium oxide (K2O) at 5 to 20 wt %;
one or more of sodium fluoride (NaF), calcium fluoride (CaF2), or aluminum fluoride (AlF3) at 1 to 5 wt %;
one or more of magnesium oxide (MgO), barium oxide (BaO), or calcium oxide (CaO) at 1 to 35 wt %; and
one or more of titanium dioxide (TiO2), cerium dioxide (CeO2), molybdenum trioxide (MoO3), bismuth oxide (Bi2O3), or copper oxide (CuO) at 10 to 25 wt %, wherein when both the MoO3 and the Bi2O3 are included, any one of the MoO3 or the Bi2O3 is included at 2 wt % or less.;
melting the materials; and
quenching the melted materials in a quenching roller to form the enamel composition.

### Claim 2 (depends on 1)

The method of claim 1, wherein the materials further include:
aluminum oxide (Al2O3) at 1 to 20 wt %;
zirconium dioxide (ZrO2) at 1 to 5 wt %; and
one or more of tin oxide (SnO) or zinc oxide (ZnO) at 1 to 10 wt %.

### Claim 3 (depends on 1)

The method in claim 1, wherein the melting of the materials for the enamel composition includes melting the materials at about 1,200 to 1,400° C. for about one to two hours.

### Claim 4 (depends on 3)

The method in claim 3, wherein the melting of the materials for the enamel composition includes melting the materials at about 1,300° C. for about 1.5 hours.

### Claim 5 (depends on 1)

The method of claim 1, wherein the quenching of the melted material includes quenching the melted materials using a quenching roller.

### Claim 6 (depends on 1)

The method of claim 1, further comprising:
applying the enamel composition to at least one of an inner surface of a cavity of a cooking appliance or an inner surface a door of the cooking appliance.

### Claim 7 (depends on 6)

The method of claim 6, wherein the applying of the enamel composition includes applying the enamel composition by a dry process that includes dispersing the quenched materials for the enamel composition in an organic binder, milling the quenched materials for the enamel composition and the organic binder to prepare a frit, and applying the frit to the at least one of the inner surface of the cavity of the cooking appliance or the inner surface the door of the cooking appliance.

### Claim 8 (depends on 6)

The method of claim 6, wherein the applying of the enamel composition includes applying the enamel composition by a wet process that includes dispersing the quenched materials for the enamel composition in water and a pigment, milling the materials for the enamel composition, water, and the pigment to prepare a frit, and applying the frit to the at least one of the inner surface of the cavity of the cooking appliance or the inner surface the door of the cooking appliance.

### Claim 9 (depends on 6)

The method of claim 6, wherein the applying of the enamel composition includes:
spraying a frit that includes the quenched materials for the enamel composition to the at least one of the inner surface of the cavity of the cooking appliance or the inner surface the door of the cooking appliance; and
firing the sprayed frit.

### Claim 10 (depends on 9)

The method of claim 9, wherein the spraying of the frit includes spraying about 300 g/m2 of the frit onto a steel sheet substrate.

### Claim 11

The method of 9, wherein the spraying of the frit includes directly applying a single layer of the frit onto a steel sheet substrate without using an interposing buffer layer, and wherein the frit is applied to form a coating layer having a thickness of about to 250 μm, and the frit is fired at about 830 to 870° C. for about 300 to 450 seconds.