# US 2023/0420654 A1 · Modified ternary and lithium manganese iron phosphate composite material and preparation method and application thereof

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2023/0420654 A1
- Document ID: US20230420654A1
- Status: Published application
- Kind: A1
- Application number: 18/464,281
- Filed: 2023-09-11
- Published: 2023-12-28
- Earliest claimed: 2022-12-21
- Assignees: Eve Power Co., Ltd.
- Applicants: Eve Power Co., Ltd.
- Inventors: TINGTING WU; LIN ZHANG; DINGDING YUAN
- Web page: https://patentgrep.com/patent/US20230420654A1

## CPC

- H01M 4/364: {as mixtures}
- C01B 25/45: containing plural metal, or metal and ammonium
- C01G 23/005: {Alkali titanates}
- H01M 4/0471: {involving thermal treatment, e.g. firing, sintering, backing particulate active material, thermal decomposition, pyrolysis}
- H01M 4/136: Electrodes based on inorganic compounds other than oxides or hydroxides, e.g. sulfides, selenides, tellurides, halogenides or LiCoFy
- H01M 4/366: {as layered products}
- H01M 4/485: of mixed oxides or hydroxides for inserting or intercalating light metals, e.g. LiTi2O4 or LiTi2OxFy (H01M4/505, H01M4/525 take precedence)
- H01M 4/505: of mixed oxides or hydroxides containing manganese for inserting or intercalating light metals, e.g. LiMn2O4 or LiMn2OxFy
- H01M 4/525: of mixed oxides or hydroxides containing iron, cobalt or nickel for inserting or intercalating light metals, e.g. LiNiO2, LiCoO2 or LiCoOxFy
- H01M 4/5825: {Oxygenated metallic salts or polyanionic structures, e.g. borates, phosphates, silicates, olivines}
- H01M 10/0525: Rocking-chair batteries, i.e. batteries with lithium insertion or intercalation in both electrodes; Lithium-ion batteries
- C01P 2002/54: one element only
- C01P 2002/72: by d-values or two theta-values, e.g. as X-ray diagram
- C01P 2004/03: obtained by SEM
- C01P 2004/61: Micrometer sized, i.e. from 1-100 micrometer
- C01P 2006/40: Electric properties
- H01M 2004/021: {Physical characteristics, e.g. porosity, surface area}
- H01M 2004/028: {Positive electrodes}
- Y02E 60/10: Energy storage using batteries
- H01M: PROCESSES OR MEANS, e.g. BATTERIES, FOR THE DIRECT CONVERSION OF CHEMICAL ENERGY INTO ELECTRICAL ENERGY
- C01B: NON-METALLIC ELEMENTS; COMPOUNDS THEREOF; {METALLOIDS OR COMPOUNDS THEREOF NOT COVERED BY SUBCLASS C01C}
- C01G: COMPOUNDS CONTAINING METALS NOT COVERED BY SUBCLASSES C01D OR C01F (metal hydrides {monoborane, diborane or addition complexes thereof} C01B6/00; salts of oxyacids of halogens C01B11/00; peroxides, salts or peroxyacids C01B15/00; thiosulfates, dithionites, polythionates C01B17/64; compounds containing selenium, or tellurium C01B19/00; binary compounds of nitrogen with metals C01B21/06; azides C01B21/08; {compounds containing nitrogen, other non-metals and metal C01B21/082}; metal amides C01B21/092; nitrites C01B21/50; {compounds of noble gases C01B23/0005}; phosphides C01B25/08; salts of oxyacids of phosphorus C01B25/16; carbides C01B32/90; compounds containing silicon C01B33/00; compounds containing boron C01B35/00; compounds having molecular sieve properties but not having base-exchange properties C01B37/00; compounds having molecular sieve and base-exchange properties, e.g. crystalline zeolites, C01B39/00; cyanides C01C3/08; salts of cyanamide C01C3/16; thiocyanates C01C3/20)
- C01P: INDEXING SCHEME RELATING TO STRUCTURAL AND PHYSICAL ASPECTS OF SOLID INORGANIC COMPOUNDS
- Y02E: REDUCTION OF GREENHOUSE GAS [GHG] EMISSIONS, RELATED TO ENERGY GENERATION, TRANSMISSION OR DISTRIBUTION

## Abstract

The present disclosure relates to a modified ternary and lithium manganese iron phosphate composite material and a preparation method and an application thereof. The material includes a modified ternary material and a modified lithium manganese iron phosphate material that are composite; wherein the modified ternary material includes a ternary material, a ternary material double-layer cladding layer, and ternary material doped metal ions; the ternary material double-layer cladding layer includes a ternary material metal oxide layer and a ternary material cationic cladding layer; the modified lithium manganese iron phosphate material includes a lithium manganese iron phosphate material, a lithium manganese iron phosphate double-layer cladding layer, and lithium manganese iron phosphate doped metal ions; the lithium manganese iron phosphate double-layer cladding layer includes a lithium manganese iron phosphate metal oxide layer and a lithium manganese iron phosphate cationic cladding layer.

## Claims

### Claim 1

A modified ternary and lithium manganese iron phosphate composite material, comprising a modified ternary material and a modified lithium manganese iron phosphate material that are composite;
wherein the modified ternary material comprises a ternary material, a ternary material double-layer cladding layer, and ternary material doped metal ions; the ternary material double-layer cladding layer comprises a ternary material metal oxide layer and a ternary material cationic cladding layer;
the modified lithium manganese iron phosphate material comprises a lithium manganese iron phosphate material, a lithium manganese iron phosphate double-layer cladding layer, and lithium manganese iron phosphate doped metal ions; the lithium manganese iron phosphate double-layer cladding layer comprises a lithium manganese iron phosphate metal oxide layer and a lithium manganese iron phosphate cationic cladding layer.

### Claim 2 (depends on 1)

The modified ternary and lithium manganese iron phosphate composite material according to claim 1, wherein a material of the ternary material metal oxide layer comprises titanium dioxide;
a material of the ternary material cationic cladding layer comprises lithium titanate;
the ternary material doped metal ions are titanium ions;
a thickness of the ternary material double-layer cladding layer is 6˜10 nm;
a material of the lithium manganese iron phosphate metal oxide layer comprises titanium dioxide;
a material of the lithium manganese iron phosphate cationic cladding layer comprises lithium titanate;
the lithium manganese iron phosphate doped metal ions are titanium ions;
a thickness of the lithium manganese iron phosphate double-layer cladding layer is 6˜10 nm.

### Claim 3 (depends on 1)

The modified ternary and lithium manganese iron phosphate composite material according to claim 1, wherein a composite mass ratio of the modified ternary material and the modified lithium manganese iron phosphate material is (0˜1):1 and is not zero;
a median particle size of the modified ternary and lithium manganese iron phosphate composite material is 215 km.

### Claim 4 (depends on 3)

The modified ternary and lithium manganese iron phosphate composite material according to claim 3, wherein a material of the ternary material metal oxide layer comprises titanium dioxide;
a material of the ternary material cationic cladding layer comprises lithium titanate;
the ternary material doped metal ions are titanium ions;
a thickness of the ternary material double-layer cladding layer is 6˜10 nm;
a material of the lithium manganese iron phosphate metal oxide layer comprises titanium dioxide;
a material of the lithium manganese iron phosphate cationic cladding layer comprises lithium titanate;
the lithium manganese iron phosphate doped metal ions are titanium ions;
a thickness of the lithium manganese iron phosphate double-layer cladding layer is 6˜10 nm.

### Claim 5 (depends on 1)

A method for preparing the modified ternary and lithium manganese iron phosphate composite material according to claim 1, comprising:
providing the modified ternary material and the modified lithium manganese iron phosphate material; and
mixing the modified ternary material and the modified lithium manganese iron phosphate material to obtain the modified ternary and lithium manganese iron phosphate composite material.

### Claim 6 (depends on 5)

The method according to claim 5, wherein a preparation method of the modified lithium manganese iron phosphate material comprises:
mixing a lithium manganese iron phosphate precursor, a lithium source, and a titanium source, spray drying and granulating, calcining under a protective atmosphere, and obtaining the modified lithium manganese iron phosphate material;
the titanium source comprises titanium trioxide;
a mass of the titanium source is 1˜4 wt % of a mass of the lithium manganese iron phosphate precursor;
the protective atmosphere is an inert gas atmosphere;
a temperature of the calcining is 700˜800° C.;
a duration of the calcining is 8˜10 h;
the calcining is further followed by treatments of crushing, sieving, and demagnetizing.

### Claim 7 (depends on 5)

The method according to claim 5, wherein a preparation method of the modified ternary material comprises:
mixing a ternary precursor, a lithium source, and a titanium source, and sintering to obtain the modified ternary material;
a molar ratio of Ni:Co:Mn in the ternary precursor is 1:1:1˜9.5:0.25:0.25;
the lithium source comprises any one or a combination of at least two of lithium hydroxide, lithium carbonate, lithium nitrate, or lithium acetate;
the titanium source comprises titanium trioxide;
a mass of the titanium source is 1˜4 wt % of a mass of the ternary precursor;
a temperature of the sintering is 750˜950° C.;
a duration of the sintering is 10˜15 h;
the sintering is further followed by treatments of roller, jaw breaker, crushing, and demagnetization.

### Claim 8 (depends on 7)

The method according to claim 7, wherein a preparation method of the modified lithium manganese iron phosphate material comprises:
mixing a lithium manganese iron phosphate precursor, a lithium source, and a titanium source, spray drying and granulating, calcining under a protective atmosphere, and obtaining the modified lithium manganese iron phosphate material;
the titanium source comprises titanium trioxide;
a mass of the titanium source is 1˜4 wt % of a mass of the lithium manganese iron phosphate precursor;
the protective atmosphere is an inert gas atmosphere;
a temperature of the calcining is 700˜800° C.;
a duration of the calcining is 8˜10 h;
the calcining is further followed by treatments of crushing, sieving, and demagnetizing.

### Claim 9 (depends on 5)

The method according to claim 5, wherein a median particle size of the modified ternary material is 5˜20 μm;
a median particle size of the modified lithium manganese iron phosphate material is 1˜5 μm;
the mixing comprises high-energy ball milling;
a ball material ratio of the high-energy ball milling is (10˜20):1;
a rotational speed of the high-energy ball milling is 1500˜2000 rpm;
a duration of the high-energy ball milling is 1˜2 h;
a mass ratio of the modified ternary material and the modified lithium manganese iron phosphate material is (0˜1):1 and is not 0.

### Claim 10 (depends on 6)

The method according to claim 6, wherein a median particle size of the modified ternary material is 5˜20 μm;
a median particle size of the modified lithium manganese iron phosphate material is 1˜5 μm;
the mixing comprises high-energy ball milling;
a ball material ratio of the high-energy ball milling is (10˜20):1;
a rotational speed of the high-energy ball milling is 1500˜2000 rpm;
a duration of the high-energy ball milling is 1˜2 h;
a mass ratio of the modified ternary material and the modified lithium manganese iron phosphate material is (0˜1):1 and is not 0.

### Claim 11 (depends on 7)

The method according to claim 7, wherein a median particle size of the modified ternary material is 5˜20 μm;
a median particle size of the modified lithium manganese iron phosphate material is 1˜5 μm;
the mixing comprises high-energy ball milling;
a ball material ratio of the high-energy ball milling is (10˜20):1;
a rotational speed of the high-energy ball milling is 1500˜2000 rpm;
a duration of the high-energy ball milling is 1˜2 h;
a mass ratio of the modified ternary material and the modified lithium manganese iron phosphate material is (0˜1):1 and is not 0.

### Claim 12 (depends on 8)

The method according to claim 8, wherein a median particle size of the modified ternary material is 5˜20 μm;
a median particle size of the modified lithium manganese iron phosphate material is 1˜5 μm;
the mixing comprises high-energy ball milling;
a ball material ratio of the high-energy ball milling is (10˜20):1;
a rotational speed of the high-energy ball milling is 1500˜2000 rpm;
a duration of the high-energy ball milling is 1˜2 h;
a mass ratio of the modified ternary material and the modified lithium manganese iron phosphate material is (0˜1):1 and is not 0.

### Claim 13 (depends on 5)

The method according to claim 5, wherein a material of the ternary material metal oxide layer comprises titanium dioxide;
a material of the ternary material cationic cladding layer comprises lithium titanate;
the ternary material doped metal ions are titanium ions;
a thickness of the ternary material double-layer cladding layer is 6˜10 nm;
a material of the lithium manganese iron phosphate metal oxide layer comprises titanium dioxide;
a material of the lithium manganese iron phosphate cationic cladding layer comprises lithium titanate;
the lithium manganese iron phosphate doped metal ions are titanium ions;
a thickness of the lithium manganese iron phosphate double-layer cladding layer is 6˜10 nm.

### Claim 14 (depends on 5)

The method according to claim 5, wherein a composite mass ratio of the modified ternary material and the modified lithium manganese iron phosphate material is (0˜1):1 and is not zero;
a median particle size of the modified ternary and lithium manganese iron phosphate composite material is 2˜15 μm.

### Claim 15 (depends on 14)

The method according to claim 14, wherein a material of the ternary material metal oxide layer comprises titanium dioxide;
a material of the ternary material cationic cladding layer comprises lithium titanate;
the ternary material doped metal ions are titanium ions;
a thickness of the ternary material double-layer cladding layer is 6˜10 nm;
a material of the lithium manganese iron phosphate metal oxide layer comprises titanium dioxide;
a material of the lithium manganese iron phosphate cationic cladding layer comprises lithium titanate;
the lithium manganese iron phosphate doped metal ions are titanium ions;
a thickness of the lithium manganese iron phosphate double-layer cladding layer is 6˜10 nm.

### Claim 16 (depends on 1)

A battery, comprising the modified ternary and lithium manganese iron phosphate composite material according to claim 1.

### Claim 17 (depends on 16)

The battery according to claim 16, wherein a material of the ternary material metal oxide layer comprises titanium dioxide;
a material of the ternary material cationic cladding layer comprises lithium titanate;
the ternary material doped metal ions are titanium ions;
a thickness of the ternary material double-layer cladding layer is 6˜10 nm;
a material of the lithium manganese iron phosphate metal oxide layer comprises titanium dioxide;
a material of the lithium manganese iron phosphate cationic cladding layer comprises lithium titanate;
the lithium manganese iron phosphate doped metal ions are titanium ions;
a thickness of the lithium manganese iron phosphate double-layer cladding layer is 6˜10 nm.

### Claim 18 (depends on 16)

The battery according to claim 16, wherein a composite mass ratio of the modified ternary material and the modified lithium manganese iron phosphate material is (0˜1):1 and is not zero;
a median particle size of the modified ternary and lithium manganese iron phosphate composite material is 215 km.

### Claim 19 (depends on 18)

The battery according to claim 18, wherein a material of the ternary material metal oxide layer comprises titanium dioxide;
a material of the ternary material cationic cladding layer comprises lithium titanate;
the ternary material doped metal ions are titanium ions;
a thickness of the ternary material double-layer cladding layer is 6˜10 nm;
a material of the lithium manganese iron phosphate metal oxide layer comprises titanium dioxide;
a material of the lithium manganese iron phosphate cationic cladding layer comprises lithium titanate;
the lithium manganese iron phosphate doped metal ions are titanium ions;
a thickness of the lithium manganese iron phosphate double-layer cladding layer is 6˜10 nm.

### Claim 20 (depends on 1)

A cathode sheet, comprising the modified ternary and lithium manganese iron phosphate composite material according to claim 1.