# US 2023/0411724 A1 · Battery recycling

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2023/0411724 A1
- Document ID: US20230411724A1
- Status: Published application
- Kind: A1
- Application number: 18/250,136
- Filed: 2021-10-20
- Published: 2023-12-21
- Earliest claimed: 2020-10-21
- Assignees: The University of Birmingham
- Applicants: The University of Birmingham
- Inventors: Laura Louise Driscoll; Peter Raymond Slater; Paul Alexander Anderson
- Web page: https://patentgrep.com/patent/US20230411724A1

## CPC

- H01M 10/54: Reclaiming serviceable parts of waste accumulators
- C01G 53/502: containing lithium and cobalt
- C01G 53/504: with the molar ratio of nickel with respect to all the metals other than alkali metals higher than or equal to 0.5, e.g. Li(MzNixCoyMn1-x-y-z)O2 with x ≥ 0.5
- C01G 53/51: containing sodium
- C01G 53/82: Compounds containing nickel, with or without oxygen or hydrogen, and containing two or more other elements
- C22B 3/165: {with organic acids}
- C22B 7/007: {by acid leaching}
- C22B 47/0063: {with acids or salt solutions (C22B47/0072 takes precedence)}
- H01M 4/0471: {involving thermal treatment, e.g. firing, sintering, backing particulate active material, thermal decomposition, pyrolysis}
- H01M 4/505: of mixed oxides or hydroxides containing manganese for inserting or intercalating light metals, e.g. LiMn2O4 or LiMn2OxFy
- H01M 4/525: of mixed oxides or hydroxides containing iron, cobalt or nickel for inserting or intercalating light metals, e.g. LiNiO2, LiCoO2 or LiCoOxFy
- Y02P 10/20: Recycling
- Y02W 30/84: Recycling of batteries or fuel cells
- H01M: PROCESSES OR MEANS, e.g. BATTERIES, FOR THE DIRECT CONVERSION OF CHEMICAL ENERGY INTO ELECTRICAL ENERGY
- C01G: COMPOUNDS CONTAINING METALS NOT COVERED BY SUBCLASSES C01D OR C01F (metal hydrides {monoborane, diborane or addition complexes thereof} C01B6/00; salts of oxyacids of halogens C01B11/00; peroxides, salts or peroxyacids C01B15/00; thiosulfates, dithionites, polythionates C01B17/64; compounds containing selenium, or tellurium C01B19/00; binary compounds of nitrogen with metals C01B21/06; azides C01B21/08; {compounds containing nitrogen, other non-metals and metal C01B21/082}; metal amides C01B21/092; nitrites C01B21/50; {compounds of noble gases C01B23/0005}; phosphides C01B25/08; salts of oxyacids of phosphorus C01B25/16; carbides C01B32/90; compounds containing silicon C01B33/00; compounds containing boron C01B35/00; compounds having molecular sieve properties but not having base-exchange properties C01B37/00; compounds having molecular sieve and base-exchange properties, e.g. crystalline zeolites, C01B39/00; cyanides C01C3/08; salts of cyanamide C01C3/16; thiocyanates C01C3/20)
- C22B: PRODUCTION AND REFINING OF METALS (electrolytic C25); PRETREATMENT OF RAW MATERIALS
- Y02P: CLIMATE CHANGE MITIGATION TECHNOLOGIES IN THE PRODUCTION OR PROCESSING OF GOODS
- Y02W: CLIMATE CHANGE MITIGATION TECHNOLOGIES RELATED TO WASTEWATER TREATMENT OR WASTE MANAGEMENT

## Abstract

A method (2800) of selectively leaching one or more manganese-containing phases from a mixed-phase battery electrode material comprises treating (2802) the mixed-phase battery electrode material with a solution of an acid, the acid acting as both a leaching agent and a reducing agent, so as to form a manganese-containing leachate whilst leaving at least one phase of the battery electrode material unleached, wherein the acid has a pKa greater than or equal to −2. Either or both of the leachate and the remaining electrode material may then be regenerated (2806, 2808).

## Claims

### Claim at position 1

1-28. (canceled)

### Claim 29

A method of selectively leaching one or more manganese-containing phases from a mixed-phase battery electrode material, the method comprising:
treating the mixed-phase battery electrode material with a solution of an acid, the acid acting as both a leaching agent and a reducing agent, so as to form a manganese-containing leachate whilst leaving at least one phase of the battery electrode material unleached, wherein the acid has a pKa greater than or equal to −2.

### Claim 30 (depends on 29)

The method of claim 29, wherein the mixed-phase battery electrode material is a cathode material from a sodium— or lithium-ion battery having a blended cathode.

### Claim 31 (depends on 29)

The method of claim 29, wherein the acid is at least one organic acid.

### Claim 32 (depends on 29)

The method of claim 29, wherein the acid has a pKa in the range from 2 to 12.

### Claim 33 (depends on 29)

The method of claim 29, wherein the acid is ascorbic acid and the acid solution is an ascorbic acid solution with a molarity in the range from 0.25M to 1.5M.

### Claim 34 (depends on 29)

The method of claim 29, wherein the treating of the electrode material is arranged to leach out at least substantially only phases in which manganese makes up at least 20% of the transition metal content.

### Claim 35 (depends on 29)

The method of claim 29, wherein the electrode material is or comprises a blended cathode strip of LMO and a layered oxide, and wherein the treating of the electrode material is arranged to selectively leach out the LMO whilst leaving the layered oxide at least substantially intact.

### Claim 36 (depends on 29)

The method of claim 29, wherein the treating of the electrode material comprises exposing the electrode material to the acid for a period of less than ten minutes.

### Claim 37 (depends on 29)

The method of claim 29, wherein the treating of the electrode material comprises exposing the electrode material to the acid for a longer time period when treating electrode material from an end-of-life (used) battery than when treating electrode material from a quality-control rejected new battery.

### Claim 38 (depends on 29)

The method of claim 29, wherein the treating of the electrode material is performed at a temperature of between 20° C. and 90° C.

### Claim 39 (depends on 29)

The method of claim 29, wherein the electrode material comprises at least one unshredded cathode strip.

### Claim 40 (depends on 35)

The method of claim 35, wherein the method further comprises re-generating an LMO phase from the leachate, the re-generating comprising:
drying the leachate so as to form a precipitate;
grinding the precipitate; and
annealing the ground precipitate in air or another oxygen-containing atmosphere.

### Claim 41 (depends on 29)

The method of claim 29, wherein the electrode material comprises LMO or NaMO which is leached by the acid solution, and the method further comprises generating a target XNixMnyCozO2 (XNMC) phase from the leachate, where X is at least one of Li, Na, from the leachate, the generating comprising:
gravimetrically determining the amount of leached LMO or NaMO in the leachate, and, based on the gravimetrically determined amount of leached LMO or NaMO:
calculating a molar amount of a cobalt- and nickel-containing sulfate, M(SO4)—nH2O (where M=Co and Ni), required to obtain the target XNMC composition from the leachate; and
calculating a molar amount of a carbonate or hydroxide of X required to obtain the target XNMC composition from the leachate;
combining the calculated amount of M(SO4) nH2O with the leachate;
adding a molar amount of a soluble source of a cation selected to trigger the precipitation of a sulfate, so as to remove the sulfate from the leachate solution, the molar amount to add being calculated from the molar amount of M(SO4) nH2O and the Co:Ni ratio of M to the leachate solution;
drying the leachate solution so as to form a precipitate;
grinding the precipitate with the calculated amount of a carbonate or hydroxide of X; and
annealing the ground material in air or another oxygen-containing atmosphere.

### Claim 42 (depends on 29)

The method of claim 29, wherein the electrode material comprises LMO or NaMO which is leached by the acid solution, and the method further comprises generating a target XNixMnyCozO2 (XNMC) phase from the leachate, where X is at least one of Li, Na, from the leachate, the generating comprising:
gravimetrically determining the amount of leached LMO or NaMO in the leachate, and, based on the gravimetrically determined amount of leached LMO or NaMO:
calculating a molar amount of a soluble source of cobalt and nickel required to obtain the target XNMC composition from the leachate; and
calculating a molar amount of a carbonate or hydroxide of X required to obtain the target XNMC composition from the leachate;
combining the calculated amount of the soluble source of cobalt and nickel with the leachate;
adding an OH− source until a precipitate is formed;
drying the precipitate;
grinding the precipitate with the calculated amount of the carbonate or hydroxide of X; and
annealing the ground material in air or another oxygen-containing atmosphere.

### Claim 43 (depends on 42)

The method of claim 42, wherein the amount of the hydroxide added to form the precipitate is the amount of the hydroxide required to bring the solution pH to 11.

### Claim 44 (depends on 29)

The method of claim 29, further comprising:
gravimetrically determining an amount of material lost from the mixed-phase battery electrode material into the leachate; and
adding a stoichiometric amount of one or more reagents to the leachate to introduce desired metal cations, so as to generate a desired battery cathode material.

### Claim 45

A battery material regeneration method for resynthesizing a layered oxide with a composition of XNixMnyCozO2 (XNMC) or XNixCoyAlzO2 (XNCA) from a battery cathode, where X is Na, Li, or a mixture of the two, the method comprising:
obtaining an XNMC- or XNCA-containing electrode material from the battery cathode;
combining the material with an OH− source, and heating the mixture to form a precipitate of NMC(OH)2 or NCA(OH)2, as appropriate, with X going into solution;
extracting and drying the NMC(OH)2 or NCA(OH)2 precipitate;
grinding the precipitate with a gravimetrically-determined stoichiometric amount of a carbonate or hydroxide of X; and
heating the resultant powder to resynthesize XNMC or XNCA.

### Claim 46 (depends on 45)

The method of claim 45, wherein sodium hydroxide is used, and wherein the sodium hydroxide is provided as an aqueous NaOH solution with a molarity in the range from 0.5 M to 1 M.

### Claim 47

A lithium-ion and/or sodium-ion battery recycling method comprising:
obtaining battery electrode material, the battery electrode material comprising multiple phases at least one of which is manganese-containing;
treating the battery electrode material with a solution of an acid with pKa greater than or equal to ˜2, the acid acting as both a leaching agent and a reducing agent so as to form a manganese-containing leachate whilst leaving at least one phase of the battery electrode material unleached,
wherein the battery electrode material is exposed to the acid solution for a period of less than twenty minutes;
draining off the leachate; and
regenerating at least one unleached phase.

### Claim 48 (depends on 47)

The method of claim 47, wherein the unleached phase is a layered oxide, and wherein the regenerating the unleached phase comprises:
forming a hydroxide of the unleached phase;
grinding the hydroxide of the unleached phase with a stoichiometric amount of LiOH H2O for a Li-ion battery material, or NaOH H2O for a Na-ion battery material; and
heating the resultant powder to resynthesise the original phase.