# US 2023/0411609 A1 · Composite positive electrode material and preparation method and application thereof

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2023/0411609 A1
- Document ID: US20230411609A1
- Status: Published application
- Kind: A1
- Application number: 18/460,626
- Filed: 2023-09-04
- Published: 2023-12-21
- Earliest claimed: 2022-12-14
- Assignees: Eve Power Co., Ltd.
- Applicants: Eve Power Co., Ltd.
- Inventors: Shengyao WEN; Lin ZHANG; Fanfen LIU; Tingting WU
- Web page: https://patentgrep.com/patent/US20230411609A1

## CPC

- H01M 4/366: {as layered products}
- C01B 25/45: containing plural metal, or metal and ammonium
- H01M 4/36: Selection of substances as active materials, active masses, active liquids
- H01M 4/505: of mixed oxides or hydroxides containing manganese for inserting or intercalating light metals, e.g. LiMn2O4 or LiMn2OxFy
- H01M 4/525: of mixed oxides or hydroxides containing iron, cobalt or nickel for inserting or intercalating light metals, e.g. LiNiO2, LiCoO2 or LiCoOxFy
- H01M 4/58: of inorganic compounds other than oxides or hydroxides, e.g. sulfides, selenides, tellurides, halogenides or LiCoFy; of polyanionic structures, e.g. phosphates, silicates or borates
- H01M 4/5825: {Oxygenated metallic salts or polyanionic structures, e.g. borates, phosphates, silicates, olivines}
- H01M 4/60: of organic compounds
- H01M 4/62: Selection of inactive substances as ingredients for active masses, e.g. binders, fillers
- H01M 10/0525: Rocking-chair batteries, i.e. batteries with lithium insertion or intercalation in both electrodes; Lithium-ion batteries
- C01P 2006/40: Electric properties
- Y02E 60/10: Energy storage using batteries
- H01M: PROCESSES OR MEANS, e.g. BATTERIES, FOR THE DIRECT CONVERSION OF CHEMICAL ENERGY INTO ELECTRICAL ENERGY
- C01B: NON-METALLIC ELEMENTS; COMPOUNDS THEREOF; {METALLOIDS OR COMPOUNDS THEREOF NOT COVERED BY SUBCLASS C01C}
- C01P: INDEXING SCHEME RELATING TO STRUCTURAL AND PHYSICAL ASPECTS OF SOLID INORGANIC COMPOUNDS
- Y02E: REDUCTION OF GREENHOUSE GAS [GHG] EMISSIONS, RELATED TO ENERGY GENERATION, TRANSMISSION OR DISTRIBUTION

## Abstract

This disclosure provides a composite positive electrode material and a preparation method and application thereof. The method includes the following steps: (1) mixing a first lithium source, a manganese source, an iron source, and a phosphorus source with a solvent to obtain a lithium manganese iron phosphate precursor, performing thermal treatment on the lithium manganese iron phosphate to obtain lithium manganese iron phosphate powder, mixing a nickel cobalt manganese hydroxide with a second lithium source, and performing sintering treatment to obtain a nickel-cobalt-lithium manganese oxide positive electrode material; (2) mixing the lithium manganese iron phosphate powder and lithium nickel cobalt manganese oxide positive electrode material obtained in step (1) with a metal-organic framework (MOF) material, and stirring to obtain mixed powder; and (3) performing calcination treatment on the mixed powder obtained in step (2) to obtain the composite positive electrode material.

## Claims

### Claim 1

A method for preparing a composite positive electrode material, comprising the following steps:
(1) mixing a first lithium source, a manganese source, an iron source, and a phosphorus source with a solvent to obtain a lithium manganese iron phosphate precursor, performing thermal treatment on the lithium manganese iron phosphate to obtain a lithium manganese iron phosphate powder, mixing a nickel cobalt manganese hydroxide with a second lithium source, and performing sintering treatment to obtain a nickel-cobalt-lithium manganese oxide positive electrode material;
(2) mixing the lithium manganese iron phosphate (LiMnxFe1-xPO4) powder and nickel-cobalt-lithium manganese oxide (LiNiaCobMn(1-a-b)O2) positive electrode material obtained in the step (1) with a metal-organic framework (MOF) material, and stirring to obtain mixed powder; and
(3) performing calcination treatment on the mixed powder obtained in the step (2) to obtain the composite positive electrode material.

### Claim 2 (depends on 1)

The method according to claim 1, wherein the first lithium source in the step (1) comprises lithium carbonate and/or lithium dihydrogen phosphate;
optionally, the manganese source comprises any one of or a combination of at least two of manganese sulfate, manganese carbonate, manganese nitrate, manganese acetate, and manganese oxalate;
optionally, the iron source comprises iron phosphate and/or iron powder;
optionally, the phosphorus source comprises phosphoric acid and/or ammonium dihydrogen phosphate;
optionally, the solvent comprises water;
optionally, the thermal treatment is performed at a temperature ranging from 600° C. to 950° C.; and
optionally, the thermal treatment is performed for a time period ranging from 5 h to 24 h.

### Claim 3 (depends on 2)

The method according to claim 2, wherein the second lithium source in the step (1) comprises lithium hydroxide and/or lithium carbonate;
optionally, the sintering treatment is performed at a temperature ranging from 450° C. to 1000° C.; and
optionally, the sintering treatment is performed for a time period ranging from 5 h to 12 h.

### Claim 4 (depends on 1)

The method according to claim 1, wherein a chemical formula of the lithium manganese iron phosphate in step (2) is LiMnxFe1-xPO4, wherein 0<x<1;
optionally, a chemical formula of the lithium nickel cobalt manganese oxide is LiNiaCobMn(1-a-b)O2, wherein a=0.5 to 0.8, and b=0.1 to 0.2;
a mass ratio of the lithium manganese iron phosphate powder to the nickel cobalt manganese positive electrode material is 1:(0.1-10); and
optionally, the MOF material comprises any one of or a combination of at least two of IRMOFs, MILs, MOF-5, MOF-74 or ZIF-8.

### Claim 5 (depends on 1)

The preparation method according to claim 1, wherein the stirring in the step (2) is performed at a speed ranging from 300 rpm to 800 rpm; and
optionally, the stirring is performed for a time period ranging from 0.5 h to 5 h.

### Claim 6 (depends on 1)

The method according to claim 1, wherein the calcination treatment in the step (3) is performed at a temperature ranging from 200° C. to 600° C.; and
optionally, the calcination treatment is performed for a time period ranging from 2 h to 12 h.

### Claim 7 (depends on 2)

The method according to claim 2, wherein the second lithium source in the step (1) comprises lithium hydroxide and/or lithium carbonate;
optionally, the sintering treatment is performed at a temperature ranging from 450° C. to 1000° C.; and
optionally, the sintering treatment is performed for a time period ranging from 5 h to 12 h.

### Claim 8 (depends on 2)

The method according to claim 2, wherein a chemical formula of the lithium manganese iron phosphate in step (2) is LiMnxFe1-xPO4, wherein 0<x<1;
optionally, a chemical formula of the lithium nickel cobalt manganese oxide is LiNiaCobMn(1-a-b)O2, wherein a=0.5 to 0.8, and b=0.1 to 0.2;
a mass ratio of the lithium manganese iron phosphate powder to the nickel cobalt manganese positive electrode material is 1:(0.1-10); and
optionally, the MOF material comprises any one of or a combination of at least two of IRMOFs, MILs, MOF-5, MOF-74 or ZIF-8.

### Claim 9 (depends on 3)

The method according to claim 3, wherein a chemical formula of the lithium manganese iron phosphate in step (2) is LiMnxFe1-xPO4, wherein 0<x<1;
optionally, a chemical formula of the lithium nickel cobalt manganese oxide is LiNiaCobMn(1-a-b)O2, wherein a=0.5 to 0.8, and b=0.1 to 0.2;
a mass ratio of the lithium manganese iron phosphate powder to the nickel cobalt manganese positive electrode material is 1:(0.1-10); and
optionally, the MOF material comprises any one of or a combination of at least two of IRMOFs, MILs, MOF-5, MOF-74 or ZIF-8.

### Claim 10 (depends on 2)

The preparation method according to claim 2, wherein the stirring in the step (2) is performed at a speed ranging from 300 rpm to 800 rpm; and
optionally, the stirring is performed for a time period ranging from 0.5 h to 5 h.

### Claim 11 (depends on 3)

The preparation method according to claim 3, wherein the stirring in the step (2) is performed at a speed ranging from 300 rpm to 800 rpm; and
optionally, the stirring is performed for a time period ranging from 0.5 h to 5 h.

### Claim 12 (depends on 4)

The preparation method according to claim 4, wherein the stirring in the step (2) is performed at a speed ranging from 300 rpm to 800 rpm; and
optionally, the stirring is performed for a time period ranging from 0.5 h to 5 h.

### Claim 13 (depends on 2)

The method according to claim 2, wherein the calcination treatment in the step (3) is performed at a temperature ranging from 200° C. to 600° C.; and
optionally, the calcination treatment is performed for a time period ranging from 2 h to 12 h.

### Claim 14 (depends on 3)

The method according to claim 3, wherein the calcination treatment in the step (3) is performed at a temperature ranging from 200° C. to 600° C.; and
optionally, the calcination treatment is performed for a time period ranging from 2 h to 12 h.

### Claim 15 (depends on 4)

The method according to claim 4, wherein the calcination treatment in the step (3) is performed at a temperature ranging from 200° C. to 600° C.; and
optionally, the calcination treatment is performed for a time period ranging from 2 h to 12 h.

### Claim 16 (depends on 5)

The method according to claim 5, wherein the calcination treatment in the step (3) is performed at a temperature ranging from 200° C. to 600° C.; and
optionally, the calcination treatment is performed for a time period ranging from 2 h to 12 h.

### Claim 17 (depends on 1)

A composite positive electrode material, prepared by the method according claim 1.

### Claim 18 (depends on 17)

The composite positive electrode material according to claim 17, wherein the first lithium source in the step (1) comprises lithium carbonate and/or lithium dihydrogen phosphate;
optionally, the manganese source comprises any one of or a combination of at least two of manganese sulfate, manganese carbonate, manganese nitrate, manganese acetate, and manganese oxalate;
optionally, the iron source comprises iron phosphate and/or iron powder;
optionally, the phosphorus source comprises phosphoric acid and/or ammonium dihydrogen phosphate;
optionally, the solvent comprises water;
optionally, the thermal treatment is performed at a temperature ranging from 600° C. to 950° C.; and
optionally, the thermal treatment is performed for a time period ranging from 5 h to 24 h.

### Claim 19 (depends on 17)

The composite positive electrode material according to claim 17, wherein the composite positive electrode material comprises a core and a coating layer disposed on a surface of the inner core;
optionally, the core comprises a nickel cobalt manganese ternary positive electrode material and a lithium manganese iron phosphate positive electrode material;
optionally, the coating layer comprises an MOF material; and
optionally, based on a mass of the composite positive electrode material being 100%, a mass fraction of the coating layer ranges from 0.1% to 1.0%.

### Claim 20 (depends on 17)

A positive electrode sheet, comprising the composite positive electrode material according to claim 17.