# US 2023/0411054 A1 · R-t-b magnet and preparation method therefor

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2023/0411054 A1
- Document ID: US20230411054A1
- Status: Published application
- Kind: A1
- Application number: 18/458,290
- Filed: 2023-08-30
- Published: 2023-12-21
- Earliest claimed: 2021-03-17
- Applicants: Fujian Changting Golden Dragon Rare-Earth Co., Ltd
- Inventors: Dakun Chen; Weiguo Mou; Jiaying Huang
- Web page: https://patentgrep.com/patent/US20230411054A1

## CPC

- H01F 1/0577: {sintered}
- H01F 41/0293: {diffusion of rare earth elements, e.g. Tb, Dy or Ho, into permanent magnets}
- H01F: MAGNETS; INDUCTANCES; TRANSFORMERS; SELECTION OF MATERIALS FOR THEIR MAGNETIC PROPERTIES

## Abstract

The invention discloses an R-T-B magnet and a preparation method thereof. The R-T-B magnet comprises the following components of: ≥30.0 wt % of R, wherein R is a rare earth element; 0.1-0.3 wt % of Nb; 0.955-1.2 wt % of B; 58-69 wt % of Fe, wherein wt % is a percentage of the mass of respective component to the total mass of all components; the R-T-B magnet further comprises Co and Ti; and in the R-T-B magnet, the ratio of the mass content of Co to the total mass content of “the Nb and the Ti” is 4-10. The present invention further optimizes the coordination relationship among the components in the R-T-B magnet, which can prepare a magnet material with relatively high levels of magnetic properties such as remanence, coercivity, squareness and the like.

## Claims

### Claim 1

A R-T-B magnet, comprising the following components of:
≥30.0 wt % of R, 0.1-0.3 wt % of Nb, 0.955-1.2 wt % of B, 58-69 wt % of Fe, Co, and Ti;
wherein R is a rare earth element and wt % is a percentage of the mass of respective component to the total mass of all components; and
the ratio of the mass content of Co to the total mass content of the Nb and the Ti is 4-10.

### Claim 2 (depends on 1)

The R-T-B magnet according to claim 1, wherein:
the content of R is 30-32 wt %; and/or
the R further comprises Nd;
wherein, the content of Nd is 22-32 wt %; and/or
the R further comprises Pr and/or RH, wherein the RH is a heavy rare earth element;
wherein, the content of the Pr is 0.3 wt % or less;
wherein, the content of the RH is 3 wt % or less;
wherein, the RH comprises Tb or Dy;
when the RH comprises Tb, the content of Tb is 0.2-1.1 wt %;
when the RH comprises Dy, the content of Dy is 0.5-2.5 wt %;
wherein a ratio of the atomic percentage of RH to the atomic percentage of R is 0.1 or less.

### Claim 3 (depends on 1)

The R-T-B magnet according to claim 1, wherein:
the content of Nb is 0.15-0.25 wt %; and/or
the ratio of the mass content of Co to the total mass content of “the Nb and the Ti” is 4.6-8.4; and/or
the content of Co is 1.5-3.5 wt %; and/or
the content of Ti is 0.15-0.35 wt %.

### Claim 4 (depends on 1)

The R-T-B magnet according to claim 1, wherein:
the content of B is 0.955-1.1 wt %; and/or
the ratio of the atomic percentage of B to the atomic percentage of R in the R-T-B magnet is 0.38 or more; and/or
the content of the Fe is 65-66 wt %; and/or
the R-T-B magnet further comprises Cu;
wherein, the content of Cu is 0.1-0.4 wt %.

### Claim 5 (depends on 1)

The R-T-B magnet according to claim 1, wherein the R-T-B magnet further comprises:
a Co—Ti—Nb phase located in an intergranular triangular region, and a ratio of the area of the Co—Ti—Nb phase in the intergranular triangular region to the total area of the intergranular triangular region is 1.1-2.5%; and
wherein the Co—Ti—Nb phase is a Co8Ti1Nb1 phase.

### Claim 6 (depends on 1)

The R-T-B magnet according to claim 1, wherein:
the R-T-B magnet comprises the following components of: 29.5 wt % of Nd, 1.1 wt % of Tb, 0.36 wt % of Cu, 2.6 wt % of Co, 0.18 wt % of Ti, 0.2 wt % of Nb, 0.99 wt % of B and 65.07 wt % of Fe, wherein wt % is the ratio of the mass of respective component to the total mass of all components; the R-T-B magnet comprises a Co8Ti1Nb1 phase in an intergranular triangular region thereof; and the ratio of the area of the Co8Ti1Nb1 phase to the total area of the intergranular triangular region is 2%; or
the R-T-B magnet comprises the following components of: 29.5 wt % of Nd, 1.1 wt % of Tb, 0.36 wt % of Cu, 2.6 wt % of Co, 0.23 wt % of Ti, 0.24 wt % of Nb, 0.99 wt % of B and 64.98 wt % of Fe, wherein wt % is the ratio of the mass of respective component to the total mass of all components; the R-T-B magnet comprises a Co8Ti1Nb1 phase in an intergranular triangular region thereof; and the ratio of the area of the Co8Ti1Nb1 phase to the total area of the intergranular triangular region is 1.8%; or
the R-T-B magnet comprises the following components of: 29.5 wt % of Nd, 1.1 wt % of Tb, 0.36 wt % of Cu, 2.6 wt % of Co, 0.35 wt % of Ti, 0.22 wt % of Nb, 0.99 wt % of B and 64.88 wt % of Fe, wherein wt % is the ratio of the mass of respective component to the total mass of all components; the R-T-B magnet comprises a Co8Ti1Nb1 phase in an intergranular triangular region thereof; and the ratio of the area of the Co8Ti1Nb1 phase to the total area of the intergranular triangular region is 1.7%; or
the R-T-B magnet comprises the following components of: 29.5 wt % of Nd, 1.1 wt % of Tb, 0.36 wt % of Cu, 2.6 wt % of Co, 0.15 wt % of Ti, 0.16 wt % of Nb, 0.99 wt % of B and 65.14 wt % of Fe, wherein wt % is the ratio of the mass of respective component to the total mass of all components; the R-T-B magnet comprises a Co8Ti1Nb1 phase in an intergranular triangular region thereof; and the ratio of the area of the Co8Ti1Nb1 phase to the total area of the intergranular triangular region is 1.5%; or
the R-T-B magnet comprises the following components of: 29.5 wt % of Nd, 1.1 wt % of Tb, 0.36 wt % of Cu, 3 wt % of Co, 0.18 wt % of Ti, 0.2 wt % of Nb, 0.99 wt % of B and 64.67 wt % of Fe, wherein wt % is the ratio of the mass of respective component to the total mass of all components; the R-T-B magnet comprises a Co8Ti1Nb1 phase in an intergranular triangular region thereof; and the ratio of the area of the Co8Ti1Nb1 phase to the total area of the intergranular triangular region is 2%; or
the R-T-B magnet comprises the following components of: 29.8 wt % of Nd, 0.8 wt % of Tb, 0.3 wt % of Cu, 2.6 wt % of Co, 0.18 wt % of Ti, 0.2 wt % of Nb, 0.99 wt % of B and 65.13 wt % of Fe, wherein wt % is the ratio of the mass of respective component to the total mass of all components; the R-T-B magnet comprises a Co8Ti1Nb1 phase in an intergranular triangular region thereof; and the ratio of the area of the Co8Ti1Nb1 phase to the total area of the intergranular triangular region is 1.9%; or
the R-T-B magnet comprises the following components of: 29.9 wt % of Nd, 0.6 wt % of Tb, 0.25 wt % of Cu, 2.5 wt % of Co, 0.18 wt % of Ti, 0.2 wt % of Nb, 0.99 wt % of B and 65.38 wt % of Fe, wherein wt % is the ratio of the mass of respective component to the total mass of all components; the R-T-B magnet comprises a Co8Ti1Nb1 phase in an intergranular triangular region thereof; and the ratio of the area of the Co8Ti1Nb1 phase to the total area of the intergranular triangular region is 2%; or
the R-T-B magnet comprises the following components of: 30.3 wt % of Nd, 0.2 wt % of Tb, 0.39 wt % of Cu, 2.8 wt % of Co, 0.23 wt % of Ti, 0.2 wt % of Nb, 0.99 wt % of B and 64.89 wt % of Fe, wherein wt % is the ratio of the mass of respective component to the total mass of all components; the R-T-B magnet comprises a Co8Ti1Nb1 phase in an intergranular triangular region thereof; and the ratio of the area of the Co8Ti1Nb1 phase to the total area of the intergranular triangular region is 1.8%; or
the R-T-B magnet comprises the following components of: 28.2 wt % of Nd, 2.5 wt % of Dy, 0.15 wt % of Cu, 3 wt % of Co, 0.25 wt % of Ti, 0.2 wt % of Nb, 0.99 wt % of B and 64.71 wt % of Fe, wherein wt % is the ratio of the mass of respective component to the total mass of all components; the R-T-B magnet comprises a Co8Ti1Nb1 phase in an intergranular triangular region thereof; and the ratio of the area of the Co8Ti1Nb1 phase to the total area of the intergranular triangular region is 1.8%; or
the R-T-B magnet comprises the following components of: 28.4 wt % of Nd, 0.5 wt % of Tb, 1.8 wt % of Dy, 0.1 wt % of Cu, 2.5 wt % of Co, 0.18 wt % of Ti, 0.2 wt % of Nb, 0.99 wt % of B and 65.33 wt % of Fe, wherein wt % is the ratio of the mass of respective component to the total mass of all components; the R-T-B magnet comprises a Co8Ti1Nb1 phase in an intergranular triangular region thereof; and the ratio of the area of the Co8Ti1Nb1 phase to the total area of the intergranular triangular region is 1.8%; or
the R-T-B magnet comprises the following components of: 29.4 wt % of Nd, 1.2 wt % of Dy, 0.39 wt % of Cu, 2 wt % of Co, 0.18 wt % of Ti, 0.2 wt % of Nb, 0.99 wt % of B and 65.64 wt % of Fe, wherein wt % is the ratio of the mass of respective component to the total mass of all components; the R-T-B magnet comprises a Co8Ti1Nb1 phase in an intergranular triangular region thereof; and the ratio of the area of the Co8Ti1Nb1 phase to the total area of the intergranular triangular region is 1.7%; or
the R-T-B magnet comprises the following components of: 29.2 wt % of Nd, 0.8 wt % of Tb, 0.6 wt % of Dy, 0.36 wt % of Cu, 2.6 wt % of Co, 0.18 wt % of Ti, 0.2 wt % of Nb, 0.99 wt % of B and 65.07 wt % of Fe, wherein wt % is the ratio of the mass of respective component to the total mass of all components; the R-T-B magnet comprises a Co8Ti1Nb1 phase in an intergranular triangular region thereof; and the ratio of the area of the Co8Ti1Nb1 phase to the total area of the intergranular triangular region is 1.6%; or
the R-T-B magnet comprises the following components of: 29.3 wt % of Nd, 0.2 wt % of Pr, 1.1 wt % of Tb, 0.36 wt % of Cu, 2.6 wt % of Co, 0.18 wt % of Ti, 0.2 wt % of Nb, 0.99 wt % of B and 65.07 wt % of Fe, wherein wt % is the ratio of the mass of respective component to the total mass of all components; the R-T-B magnet comprises a Co8Ti1Nb1 phase in an intergranular triangular region thereof; and the ratio of the area of the Co8Ti1Nb1 phase to the total area of the intergranular triangular region is 1.7%; or
the R-T-B magnet comprises the following components of: 29.5 wt % of Nd, 1.1 wt % of Tb, 0.36 wt % of Cu, 2.6 wt % of Co, 0.18 wt % of Ti, 0.2 wt % of Nb, 0.99 wt % of B and 65.07 wt % of Fe, wherein wt % is the ratio of the mass of respective component to the total mass of all components; the R-T-B magnet comprises a Co8Ti1Nb1 phase in an intergranular triangular region thereof; and the ratio of the area of the Co8Ti1Nb1 phase to the total area of the intergranular triangular region is 1.2%; or
the R-T-B magnet comprises the following components of: 29.5 wt % of Nd, 1.1 wt % of Tb, 0.36 wt % of Cu, 2.6 wt % of Co, 0.18 wt % of Ti, 0.2 wt % of Nb, 0.99 wt % of B and 65.07 wt % of Fe, wherein wt % is the ratio of the mass of respective component to the total mass of all components; the R-T-B magnet comprises a Co8Ti1Nb1 phase in an intergranular triangular region thereof; and the ratio of the area of the Co8Ti1Nb1 phase to the total area of the intergranular triangular region is 1.1%.

### Claim 7 (depends on 1)

A preparation method of a R-T-B magnet, comprising the steps of subjecting a raw mixture comprising the respective components for the R-T-B magnet according to claim 1 to a smelting treatment, an air cooling treatment and an aging treatment in turn.

### Claim 8 (depends on 7)

The preparation method of the R-T-B magnet according to claim 7, wherein:
the temperature for the sintering treatment is 1000-1100° C.; and/or
the time for the sintering treatment is 4-8 h; and/or
the temperature for the air cooling treatment is 550-950° C.; and/or
the aging treatment comprises a primary aging treatment and a secondary aging treatment;
wherein the temperature for the primary aging treatment is 860-920° C.;
wherein the time for the primary aging treatment is 2.5-4 h;
wherein the temperature for the secondary aging treatment is 460-530° C.;
wherein the time for the secondary aging treatment is 2.5-4 h; and/or
wherein, when the R-T-B magnet comprises a heavy rare earth element, the preparation method further comprises a grain boundary diffusion after the aging treatment;
wherein, the temperature for the grain boundary diffusion is 800-900° C.;
wherein, the time for the grain boundary diffusion is 5-10 h;
wherein, the method of adding heavy rare earth elements in the R-T-B magnet comprises the steps of adding 0-80% of heavy rare earth elements during the smelting and adding the remaining heavy rare earth elements during the grain boundary diffusion; when the heavy rare earth elements in the R-T-B magnet are Tb with a content of greater than 0.5 wt %, 25-67% of Tb is added during the smelting, and the rest is added during the grain boundary diffusion; or, when the heavy rare earth elements in the R-T-B magnet are Tb and Dy, the Tb is added during smelting, and the Dy is added during the grain boundary diffusion; or when the heavy rare earth elements in the R-T-B magnet are Tb with a content of less than or equal to 0.5 wt %, or when the heavy rare earth elements in the R-T-B magnet are Dy, the heavy rare earth elements in the R-T-B magnet are added during the grain boundary diffusion.

### Claim 9 (depends on 7)

The preparation method of the R-T-B magnet according to claim 7, wherein the preparation method further comprises the steps of smelting, casting, hydrogen decrepitation, pulverization and shaping treatment before the sintering treatment,
wherein, the temperature for the smelting is 1550° C. or less;
wherein, the temperature for the casting is 1410-1440° C.;
wherein, the alloy sheet obtained after the casting has a thickness of 0.25-0.40 mm;
wherein, the process of the hydrogen decrepitation comprises hydrogen absorption, dehydrogenation, and a cooling treatment in turn;
wherein, the magnetic field strength for the magnetic field shaping is 1.8 T or more.

### Claim 10 (depends on 1)

A R-T-B magnet prepared by the preparation method of the R-T-B magnet according to claim 1.

### Claim 11 (depends on 2)

The R-T-B magnet according to claim 2, wherein the R-T-B magnet further comprises a Co—Ti—Nb phase; the Co—Ti—Nb phase is located in an intergranular triangular region, and a ratio of the area of the Co—Ti—Nb phase in the intergranular triangular region to the total area of the intergranular triangular region is 1.1-2.5%; and
wherein the Co—Ti—Nb phase is a Co8Ti1Nb1 phase.

### Claim 12 (depends on 3)

The R-T-B magnet according to claim 3, wherein the R-T-B magnet further comprises a Co—Ti—Nb phase; the Co—Ti—Nb phase is located in an intergranular triangular region, and a ratio of the area of the Co—Ti—Nb phase in the intergranular triangular region to the total area of the intergranular triangular region is 1.1-2.5%; and
wherein the Co—Ti—Nb phase is a Co8Ti1Nb1 phase.

### Claim 13 (depends on 4)

The R-T-B magnet according to claim 4, wherein the R-T-B magnet further comprises a Co—Ti—Nb phase; the Co—Ti—Nb phase is located in an intergranular triangular region, and a ratio of the area of the Co—Ti—Nb phase in the intergranular triangular region to the total area of the intergranular triangular region is 1.1-2.5%; and
wherein the Co—Ti—Nb phase is a Co8Ti1Nb1 phase.